I don't normally photograph an entire project, but seeing as I had some free sample prepregs from 2 different suppliers I thought I'd turn it into a giggle. They both know I use VTF, and they assured me that their materials would compete. They told me that although the materials are made for autoclave, that I should see promising results OOA. I didnt get my hopes up as Ive tried several before and they all sucked. I thought I'd turn it into a simple little project to play with these samples. The idea was to take a wooden part (as wood is something I haven't replicated before) that had a simple shape (I didn't have much hope for snything that isnt VTF). Nothing that would take longer than a week. So here it is, from original part to polished carbon copy: Original wood part:


I tryed using teak oil to seal it, but that didnt work, it just kept sucking the oil, grain was still open.


So I used aluminium tape:

Flanges:


I knew I was gonna have to sand the stripes left by the aluminium tape, so i took the safest route which was to take a mould off the B side, this would in turn become a plug which I could sand down, most likely sanding the gelcoat quite thin. If I sand too far into the gelcoat, I dont have to worry as I will be taking a proper mould off it later. So making of the plug, followed by the mould:











Sanded the lines down with a block, and tried to get rid of negatives on the flanges. You can see why I did it this way, the grey spot there is where I sanded through the gelcoat into the skin coat, theres other spots like it and you can start to see the grey show through the green:





Postcure:

Taking the ali off was a right bitch, and it left a residue which was even harder to take off. Next time, Ill find a better way to do this:

To the prepreg room! Sealed and released:

Thawing and cutting the material:


Layup:


Bagging:






Bake:

Fresh out the oven:


Releasing was this easy:


Oh dear, it seems there was a bit of bridging. Im not surprised. As Iv'e said before, nothing beats VTF. These two photos were sent straight to the sales rep. Hes sending another sample :


No carbon is scarp though, so I battled on. My plan was to fill the voids, mask them and put black stripes at the ends:





Sanding:

Some peeps on here get paranoid about fillinf the pinholes and voids with dust. Its nothing to worry about, the dust is transparent, and a layer of clear will make it dissapear:


Before the next coat, I'll try something new, branding. I've got a vinyl cutter, plus I made all of my branding myself, so I have the vector files, seemed rude not to do it:




The masking didnt really work, but I think it looks quite cool, even if by accident:

So, more sanding and lacquering, until the pinholes were filled, now go up the grades 400, 600, 800, 1200, 1500, 3000 then compounds coarse then fine:




Finished product on my desk:

Determined not to be beat, I remembered the second sample I had. Along with some new found knowledge gained from this paper:
http://digitool.library.mcgill.ca/webclient/StreamGate?folder_id=0&dvs=1371902526959~725
You could read the whole thing, or I could summarize it to this: DONT USE BREATHER!









 As simple as it is, I did learn something. If youre making a part out of wood, don't use ali tape. Two reasons. First, You have to sand back the gelcoat to get the lines off, and hence making your mould weaker (unless you did the plug-mould method I did. And second, if the original is not sacrificial, youre going to have a hard time taking the ali and its adhesive off very carefully. WD40 got it off without staining it, but I wouldnt place a bet if it was a different wood that was untreated.
I will also be commencing production without breather on the part, just on the mould.
Overall good experience, and the tea tray sold for £150 (for a weeks work!). Hopefully you guys can take something from it too.
|
Group: Forum Members
Posts: 243,
Visits: 1K
|
morepower (24/06/2013) I use pre-preg Diolen ... I need some prepreg Diolen sharpish. Just emailed PRF for a quote on a 25m roll, but only need about 5 metres. Let me know if you wanna do a group buy. I'm gonna have to get a roll of VTF as well soon.... How are you doing for VTF?
|
Group: Forum Members
Posts: 242,
Visits: 1.2K
|
carboncactus (24/06/2013)
morepower (24/06/2013) I use pre-preg Diolen ... I need some prepreg Diolen sharpish. Just emailed PRF for a quote on a 25m roll, but only need about 5 metres. Let me know if you wanna do a group buy. I'm gonna have to get a roll of VTF as well soon.... How are you doing for VTF? Bear with me...lol... I have a little issue with a customer of our mutual friend.... he paid for a kit direct to ****s and then didnt want to pay more... Now he does.. so it is an on/off/on sale so as he didnt want the kit I sold it as it was taking up space... So it looks like I will need some more...Of both..... PRF will do 5m but I may need a couple of meters too so if we get a 10m roll and split it. It might be perfect..... I have to check how much VTF I have....
|
Group: Forum Members
Posts: 243,
Visits: 1K
|
morepower (25/06/2013) PRF will do 5m but I may need a couple of meters too so if we get a 10m roll and split it. It might be perfect..... I have to check how much VTF I have.... Which resin system and Diolen weight would it be? I quoted for 25m of 265g on RF464 (low temp)
|
Group: Forum Members
Posts: 242,
Visits: 1.2K
|
carboncactus (25/06/2013)
morepower (25/06/2013) PRF will do 5m but I may need a couple of meters too so if we get a 10m roll and split it. It might be perfect..... I have to check how much VTF I have.... Which resin system and Diolen weight would it be? I quoted for 25m of 265g on RF464 (low temp) That is fine.. It is the stuff I used last time with the VTF suface and the SHD backing material and it was compatible with both..
|