Weird fiberglass panel issue


Author
Message
raygun
r
Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)
Group: Forum Members
Posts: 22, Visits: 126
I'm getting ready to make a mold from the hood of my 2011 Corvette. When I bought the car in April, it had a weird matte vinyl wrap on the hood. When I removed said wrap (ugh), I found an odd grid of what I thought, at the time, were scratches.
Since I've finally found time to get started on the planned carbon hood with some heat extraction, I took a closer look at the hood. These don't really look like scratches so much as CSM. They also line up with the reinforcement on the bottom of the panel.
I cannot, for the life of me, figure out what could possibly cause this. I posted a question on one of the Facebook groups. It turns out that a lot of Corvette owners have this issue, in the pattern and same places on the hood. Someone suggested that it may be related to heat from storing the car in direct sunlight. That strikes me as weird.




And on someone else's car:

I love the car, but... lovely GM quality strikes again.
Any ideas what could cause this? Also, I'm worried that buffing and preparing the surface may just make it worse. I'd appreciate any advice y'all might have  as to cause and possible solutions. I'd really like to clean this up before making a mold.

Edited 5 Years Ago by raygun
Replies
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
It's print through from where the inner skin is bonded to the outer skin, the adhesive will cause distortions like this. Actually even occurs on metal panels, if you look closely enough at most cars with bonded panels (roof being the easiest to spot) you will probably find where the adhesive has creased the sheet metal. 
raygun
r
Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)
Group: Forum Members
Posts: 22, Visits: 126
Hanaldo - 11/19/2020 9:00:14 PM
It's print through from where the inner skin is bonded to the outer skin, the adhesive will cause distortions like this. Actually even occurs on metal panels, if you look closely enough at most cars with bonded panels (roof being the easiest to spot) you will probably find where the adhesive has creased the sheet metal. 

Thanks!

So, how do I keep this from happening on my own piece? This will be my first carbon project, and my first two-piece mold. I've watched all of the (amazing!) Easy Composites videos and I've made a few fiberglass parts, but they were all pretty much lofted 2D shapes that didn't require any sort of reinforcement. This piece is about 42" x 30". I don't expect it to be show-car quality (gotta start somewhere!) but I'd rather not have this problem. 

Can I assume that, if the inner and outer parts are bonded with resin rather than some weird adhesive, this won't be an issue?

(Hello from the nice part of Texas!)

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
raygun - 5 Years Ago
Warren (Staff) - 5 Years Ago
raygun - 5 Years Ago
Hanaldo - 5 Years Ago
raygun - 5 Years Ago
Hanaldo - 5 Years Ago
raygun - 5 Years Ago
Hanaldo - 5 Years Ago