Hi EC,

After doing my infusion practice for over than 2 years, I loved to hear from you about what I need to do to having my first touch on pre-preg composites manufacture. would you please make a price list about the equipment of pre-preg (autoclaved/composites oven, pre-preg, storage chamber, etc". autoclaved seems like a spooky price tag, could we subtitute the fuction with curing oven?

Hope hear from you

Leon
Reply
Matt (Staff)
Matt (Staff)
Composites Expert (Staff) (8.5K reputation)Composites Expert (Staff) (8.5K reputation)Composites Expert (Staff) (8.5K reputation)Composites Expert (Staff) (8.5K reputation)Composites Expert (Staff) (8.5K reputation)Composites Expert (Staff) (8.5K reputation)Composites Expert (Staff) (8.5K reputation)Composites Expert (Staff) (8.5K reputation)Composites Expert (Staff) (8.5K reputation)
Group: Forum Members
Posts: 680, Visits: 1.9K
Hi Matthieu,

Thanks for the feedback. I've fixed the typo and spent the day adding in all of the photographs to the guide. There are lots of detailed photos in there now so it should be much easier to follow. I've updated the link on the original post so if you download that you'll get the new full version of the guide.

Answers to your questions:

- How long does it takes to have the prepreg from freezer temp to room temperature?


For a small amount (1-2m) it would only take a few hours. For a full roll (like the master rolls we're cutting from) it can take 24hrs.

- I'm using maguire mirror glaze high temp mould release, would this be suitable for prepreg?


Personally, I wouldn't recommend it. Even wax listed as 'High Temperature' is not really that high temperature and I don't know anyone using traditional wax of any kind for prepregs. It's chemical release agents (like Easy-Lease) all the way.

Enjoy the guide!

Matt

Matt Statham
Easy Composites / Carbon Mods - Technical Sales
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search