Ciao a tutti,
avrei bisogno di qualche consiglio per realizzare uno stampo per un parabordo. Il parafango è in fibra di vetro e vorrei realizzarlo in fibra di carbonio.
I miei dubbi riguardano i bordi che vanno verso l'interno e quindi creano angoli negativi che impediscono la creazione di un unico stampo.
Poiché questi bordi si trovano su quasi tutti i lati del paraurti, quale pensi sia il modo giusto di procedere?

Grazie mille


Replies
AndrewL92
A
Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)
Group: Forum Members
Posts: 6, Visits: 103
Hanaldo - 11/24/2020 9:57:07 PM
Oh I see, no dont do that. Resin will go everywhere and make a big mess, and you will likely still struggle to get a seal due the bolt holes.

Just run your sealant tape around the perimeter of the flange as it is and try to get it to seal like that. Good chance it won't, so then I would double bag and place the entire mould inside an envelope bag. The first bag will prevent resin from going where you dont want it, while the second will provide the seal. Just watch out for puncturing the second bag on the mould or your bolts.


Perfect, then proceed as you advised me.
In this regard, I had some questions:

1. if I use gelcoat, to make a bead between the flanges, as you advised, how long do I have to wait to close the flanges together? As soon as I apply the gelcoat?
And to proceed with the infusion?
Can i use a gelcoat additive?

2. How do I seal the bolt holes? By applying the gelcot in the hole and then screwing?

3. What reinforcement do you recommend for these fenders? Would it make sense to use lantor soric?

Thanks again for your availability
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
AndrewL92 - 11/25/2020 12:44:18 AM
Hanaldo - 11/24/2020 9:57:07 PM
Oh I see, no dont do that. Resin will go everywhere and make a big mess, and you will likely still struggle to get a seal due the bolt holes.

Just run your sealant tape around the perimeter of the flange as it is and try to get it to seal like that. Good chance it won't, so then I would double bag and place the entire mould inside an envelope bag. The first bag will prevent resin from going where you dont want it, while the second will provide the seal. Just watch out for puncturing the second bag on the mould or your bolts.


Perfect, then proceed as you advised me.
In this regard, I had some questions:

1. if I use gelcoat, to make a bead between the flanges, as you advised, how long do I have to wait to close the flanges together? As soon as I apply the gelcoat?
And to proceed with the infusion?
Can i use a gelcoat additive?

2. How do I seal the bolt holes? By applying the gelcot in the hole and then screwing?

3. What reinforcement do you recommend for these fenders? Would it make sense to use lantor soric?

Thanks again for your availability



1. Yes, bolt the flanges together as soon as you have applied the gelcoat. In all likelihood you will find the gelcoat will be starting to thicken up as you are ready to bolt the flanges on, which is perfect. As long as you get them bolted together before the gelcoat cures too hard to allow that then you're fine.

2. I generally just run a 'ring' of gelcoat around the hole and that will seal it up when you bolt the flanges together. Having a small rattlegun will make it quicker to remove the bolts when you are done as you will likely find gelcoat gets squeezed up into the threads, but even if you don't have a rattlegun its not hard, the gelcoat doesn't stick well to steel bolts.

3. Depends totally on your application. For a race car, I'd be doing a single layer of 200g and a single layer of ~400g, a bit extra in the mounting points, and thats it. For a street car, I probably still wouldn't use a core, but I would probably do 2 layers of 200g, 1 layer of a 400g Kevlar, and 1 layer of a 400g carbon.
beliblisk
b
Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)
Group: Forum Members
Posts: 53, Visits: 2.8K
Put mixed gelcoat in plastic food bag, squeeze it in one corner, twist bag around so you end up with all gelocoat trapped in one corner and then just nipp off tge corner (much like if you are baking cakes) and you will be able to apply nice lines quickly without any messSmile 

For layup you can go as low as one 200g cf followed by 200 cf/kevlar  hybrid as there is enough geometry on your side(extra 400g on the mounting points)..... for street car i normally go with 1mm in total for fenders. 




Edited 5 Years Ago by beliblisk
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
AndrewL92 - 5 Years Ago
Warren (Staff) - 5 Years Ago
AndrewL92 - 5 Years Ago
Hanaldo - 5 Years Ago
Warren (Staff) - 5 Years Ago
AndrewL92 - 5 Years Ago
Hanaldo - 5 Years Ago
beliblisk - 5 Years Ago
Hanaldo - 5 Years Ago
beliblisk - 5 Years Ago
AndrewL92 - 5 Years Ago
Hanaldo - 5 Years Ago
AndrewL92 - 5 Years Ago
Hanaldo - 5 Years Ago
AndrewL92 - 5 Years Ago
Hanaldo - 5 Years Ago
beliblisk - 5 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search