Put mixed gelcoat in plastic food bag, squeeze it in one corner, twist bag around so you end up with all gelocoat trapped in one corner and then just nipp off tge corner (much like if you are baking cakes) and you will be able to apply nice lines quickly without any messSmile 

For layup you can go as low as one 200g cf followed by 200 cf/kevlar  hybrid as there is enough geometry on your side(extra 400g on the mounting points)..... for street car i normally go with 1mm in total for fenders. 




Edited 6 Years Ago by beliblisk
Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
AndrewL92 - 11/25/2020 12:44:18 AM
Hanaldo - 11/24/2020 9:57:07 PM
Oh I see, no dont do that. Resin will go everywhere and make a big mess, and you will likely still struggle to get a seal due the bolt holes.

Just run your sealant tape around the perimeter of the flange as it is and try to get it to seal like that. Good chance it won't, so then I would double bag and place the entire mould inside an envelope bag. The first bag will prevent resin from going where you dont want it, while the second will provide the seal. Just watch out for puncturing the second bag on the mould or your bolts.


Perfect, then proceed as you advised me.
In this regard, I had some questions:

1. if I use gelcoat, to make a bead between the flanges, as you advised, how long do I have to wait to close the flanges together? As soon as I apply the gelcoat?
And to proceed with the infusion?
Can i use a gelcoat additive?

2. How do I seal the bolt holes? By applying the gelcot in the hole and then screwing?

3. What reinforcement do you recommend for these fenders? Would it make sense to use lantor soric?

Thanks again for your availability



1. Yes, bolt the flanges together as soon as you have applied the gelcoat. In all likelihood you will find the gelcoat will be starting to thicken up as you are ready to bolt the flanges on, which is perfect. As long as you get them bolted together before the gelcoat cures too hard to allow that then you're fine.

2. I generally just run a 'ring' of gelcoat around the hole and that will seal it up when you bolt the flanges together. Having a small rattlegun will make it quicker to remove the bolts when you are done as you will likely find gelcoat gets squeezed up into the threads, but even if you don't have a rattlegun its not hard, the gelcoat doesn't stick well to steel bolts.

3. Depends totally on your application. For a race car, I'd be doing a single layer of 200g and a single layer of ~400g, a bit extra in the mounting points, and thats it. For a street car, I probably still wouldn't use a core, but I would probably do 2 layers of 200g, 1 layer of a 400g Kevlar, and 1 layer of a 400g carbon.
AndrewL92
A
Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)
Group: Forum Members
Posts: 6, Visits: 103
Hanaldo - 11/24/2020 9:57:07 PM
Oh I see, no dont do that. Resin will go everywhere and make a big mess, and you will likely still struggle to get a seal due the bolt holes.

Just run your sealant tape around the perimeter of the flange as it is and try to get it to seal like that. Good chance it won't, so then I would double bag and place the entire mould inside an envelope bag. The first bag will prevent resin from going where you dont want it, while the second will provide the seal. Just watch out for puncturing the second bag on the mould or your bolts.


Perfect, then proceed as you advised me.
In this regard, I had some questions:

1. if I use gelcoat, to make a bead between the flanges, as you advised, how long do I have to wait to close the flanges together? As soon as I apply the gelcoat?
And to proceed with the infusion?
Can i use a gelcoat additive?

2. How do I seal the bolt holes? By applying the gelcot in the hole and then screwing?

3. What reinforcement do you recommend for these fenders? Would it make sense to use lantor soric?

Thanks again for your availability
Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Oh I see, no dont do that. Resin will go everywhere and make a big mess, and you will likely still struggle to get a seal due the bolt holes.

Just run your sealant tape around the perimeter of the flange as it is and try to get it to seal like that. Good chance it won't, so then I would double bag and place the entire mould inside an envelope bag. The first bag will prevent resin from going where you dont want it, while the second will provide the seal. Just watch out for puncturing the second bag on the mould or your bolts.
AndrewL92
A
Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)
Group: Forum Members
Posts: 6, Visits: 103
I'm probably saying nonsense but yes, the idea was to include the top flanges in the bag.
I made an image to make you see well.
The black lines are where I would like to cut, and the red one where I would place the taky tape.

Nonsense?
Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
AndrewL92 - 11/22/2020 12:36:22 AM
Hanaldo - 11/19/2020 12:05:18 AM
No reason why you can't use it, some of those flange shapes are going to make things challenging for you but it's certainly usable. 

You either need to seal the flanges with something before bolting them together, or you will need to envelope bag the entire thing. Envelope bagging I find quite unreliable for infusion due to the propensity for leaks, especially on larger complex moulds like this, so I try to avoid it. for sealing the flanges, the easiest and most reliable way I've found is to use an RTV silicone gasket maker (do NOT use an adhesive caulking silicone, these will bond your flanges together regardless of release agent). The downside is this is a bit difficult to clean up after the infusion, so it becomes a bit of a pain to reuse the moulds. Another way I do it is to run a 'bead' of gelcoat all around the flanges, and then bolt the flanges together before the gelcoat cures. This is significantly easier to clean up, but doesn't seal as reliably as the silicone gasket. Using either method, don't forget to seal up your bolt holes as well.

Thanks for the reply.

I understand what you said. The only doubt I have is how to arrange the taky tape all around the perimeter, without any leakage, especially where the vertical and horizontal flanges join or in other parts where there are fairly tight curves. Maybe it's my inexperience that makes me see the problem!

Another way I had thought of to proceed with the infusion was to slightly cut out the upper flanges to create a bead of a couple of cm along the entire perimeter to apply the taky tape. This way I would only have to finish the top flanges and would only need to seal the bolt holes. What do you think about it?
I hope I explained myself.

Yes that's definitely the tricky bit now, I can foresee you struggling with leaks.

I'm not sure i follow what you mean about cutting the flanges. I certainly wouldn't make them any shorter if that's what you are thinking??

AndrewL92
A
Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)Supreme Being (77 reputation)
Group: Forum Members
Posts: 6, Visits: 103
Hanaldo - 11/19/2020 12:05:18 AM
No reason why you can't use it, some of those flange shapes are going to make things challenging for you but it's certainly usable. 

You either need to seal the flanges with something before bolting them together, or you will need to envelope bag the entire thing. Envelope bagging I find quite unreliable for infusion due to the propensity for leaks, especially on larger complex moulds like this, so I try to avoid it. for sealing the flanges, the easiest and most reliable way I've found is to use an RTV silicone gasket maker (do NOT use an adhesive caulking silicone, these will bond your flanges together regardless of release agent). The downside is this is a bit difficult to clean up after the infusion, so it becomes a bit of a pain to reuse the moulds. Another way I do it is to run a 'bead' of gelcoat all around the flanges, and then bolt the flanges together before the gelcoat cures. This is significantly easier to clean up, but doesn't seal as reliably as the silicone gasket. Using either method, don't forget to seal up your bolt holes as well.

Thanks for the reply.

I understand what you said. The only doubt I have is how to arrange the taky tape all around the perimeter, without any leakage, especially where the vertical and horizontal flanges join or in other parts where there are fairly tight curves. Maybe it's my inexperience that makes me see the problem!

Another way I had thought of to proceed with the infusion was to slightly cut out the upper flanges to create a bead of a couple of cm along the entire perimeter to apply the taky tape. This way I would only have to finish the top flanges and would only need to seal the bolt holes. What do you think about it?
I hope I explained myself.

beliblisk
b
Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)
Group: Forum Members
Posts: 53, Visits: 2.8K
Hanaldo - 11/19/2020 9:02:24 PM
beliblisk - 11/19/2020 7:25:04 PM
Hanaldo - 11/19/2020 12:05:18 AM
No reason why you can't use it, some of those flange shapes are going to make things challenging for you but it's certainly usable. 

You either need to seal the flanges with something before bolting them together, or you will need to envelope bag the entire thing. Envelope bagging I find quite unreliable for infusion due to the propensity for leaks, especially on larger complex moulds like this, so I try to avoid it. for sealing the flanges, the easiest and most reliable way I've found is to use an RTV silicone gasket maker (do NOT use an adhesive caulking silicone, these will bond your flanges together regardless of release agent). The downside is this is a bit difficult to clean up after the infusion, so it becomes a bit of a pain to reuse the moulds. Another way I do it is to run a 'bead' of gelcoat all around the flanges, and then bolt the flanges together before the gelcoat cures. This is significantly easier to clean up, but doesn't seal as reliably as the silicone gasket. Using either method, don't forget to seal up your bolt holes as well.

Regarding the sealing mould parts.

Would you say that gum tape in 2mm recess integrated in the flange works better than gelcoat method?

I used RVT silicon befor but as mentioned its a pain to clean so for next multi part tool i was planning to go gum tape route.

thanks a lot

Tried it, but didn't find it very reliable. The tape tends to compress quite easily, and it often ends up that in some areas it doesn't contact the opposite flange properly and doesn't seal. It also still makes a hell of a mess, its just as hard to clean up as the silicone.

So we actually have to choose lesser evil in this case and dummy vacuum befor actually laying any of the materials.

I used gasket type rvt on custumers tools (quality wasnt the best) and i actually pulled gelcoat off the flange when demoulding...... but it held vacuum perfectlySmile

Still on the look out for better solution.

Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
beliblisk - 11/19/2020 7:25:04 PM
Hanaldo - 11/19/2020 12:05:18 AM
No reason why you can't use it, some of those flange shapes are going to make things challenging for you but it's certainly usable. 

You either need to seal the flanges with something before bolting them together, or you will need to envelope bag the entire thing. Envelope bagging I find quite unreliable for infusion due to the propensity for leaks, especially on larger complex moulds like this, so I try to avoid it. for sealing the flanges, the easiest and most reliable way I've found is to use an RTV silicone gasket maker (do NOT use an adhesive caulking silicone, these will bond your flanges together regardless of release agent). The downside is this is a bit difficult to clean up after the infusion, so it becomes a bit of a pain to reuse the moulds. Another way I do it is to run a 'bead' of gelcoat all around the flanges, and then bolt the flanges together before the gelcoat cures. This is significantly easier to clean up, but doesn't seal as reliably as the silicone gasket. Using either method, don't forget to seal up your bolt holes as well.

Regarding the sealing mould parts.

Would you say that gum tape in 2mm recess integrated in the flange works better than gelcoat method?

I used RVT silicon befor but as mentioned its a pain to clean so for next multi part tool i was planning to go gum tape route.

thanks a lot

Tried it, but didn't find it very reliable. The tape tends to compress quite easily, and it often ends up that in some areas it doesn't contact the opposite flange properly and doesn't seal. It also still makes a hell of a mess, its just as hard to clean up as the silicone.

beliblisk
b
Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)Supreme Being (811 reputation)
Group: Forum Members
Posts: 53, Visits: 2.8K
Hanaldo - 11/19/2020 12:05:18 AM
No reason why you can't use it, some of those flange shapes are going to make things challenging for you but it's certainly usable. 

You either need to seal the flanges with something before bolting them together, or you will need to envelope bag the entire thing. Envelope bagging I find quite unreliable for infusion due to the propensity for leaks, especially on larger complex moulds like this, so I try to avoid it. for sealing the flanges, the easiest and most reliable way I've found is to use an RTV silicone gasket maker (do NOT use an adhesive caulking silicone, these will bond your flanges together regardless of release agent). The downside is this is a bit difficult to clean up after the infusion, so it becomes a bit of a pain to reuse the moulds. Another way I do it is to run a 'bead' of gelcoat all around the flanges, and then bolt the flanges together before the gelcoat cures. This is significantly easier to clean up, but doesn't seal as reliably as the silicone gasket. Using either method, don't forget to seal up your bolt holes as well.

Regarding the sealing mould parts.

Would you say that gum tape in 2mm recess integrated in the flange works better than gelcoat method?

I used RVT silicon befor but as mentioned its a pain to clean so for next multi part tool i was planning to go gum tape route.

thanks a lot

Edited 6 Years Ago by beliblisk
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search