Ciao a tutti,
avrei bisogno di qualche consiglio per realizzare uno stampo per un parabordo. Il parafango è in fibra di vetro e vorrei realizzarlo in fibra di carbonio.
I miei dubbi riguardano i bordi che vanno verso l'interno e quindi creano angoli negativi che impediscono la creazione di un unico stampo.
Poiché questi bordi si trovano su quasi tutti i lati del paraurti, quale pensi sia il modo giusto di procedere?

Grazie mille


Replies
AndrewL92
A
Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)Forum Guru (53 reputation)
Group: Forum Members
Posts: 6, Visits: 103
Thanks for the reply.
I know that from a photo it is not easy to understand but do you think it will be okay if I divide the mold in this way?
Or do you suggest me to proceed differently, making more parts or dividing it differently?


Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
AndrewL92 - 9/24/2020 1:43:40 PM
Thanks for the reply.
I know that from a photo it is not easy to understand but do you think it will be okay if I divide the mold in this way?
Or do you suggest me to proceed differently, making more parts or dividing it differently?


Doing it this way will result in super obvious flash lines on the finished part, right in the middle of the cosmetic areas.

Much better to put your barriers on a radius where you can. For fenders, you generally do the main 'face' of the guard as one piece, and then each of the mounting flanges where it returns on itself can be split along the radius. So for these guards, you will likely end up with at least a 3, potentially a 4 piece mould.

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
AndrewL92 - 5 Years Ago
Warren (Staff) - 5 Years Ago
AndrewL92 - 5 Years Ago
Hanaldo - 5 Years Ago
Warren (Staff) - 5 Years Ago
AndrewL92 - 5 Years Ago
Hanaldo - 5 Years Ago
beliblisk - 5 Years Ago
Hanaldo - 5 Years Ago
beliblisk - 5 Years Ago
AndrewL92 - 5 Years Ago
Hanaldo - 5 Years Ago
AndrewL92 - 5 Years Ago
Hanaldo - 5 Years Ago
AndrewL92 - 5 Years Ago
Hanaldo - 5 Years Ago
beliblisk - 5 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search