Hi Phil.
The post-cure schedule that you have specified will provide the maximum HDT (Heat Distortion Temperature), running the post-cure to higher temperatures will not increase this figure, however, it is possible to reduce to post-curing times. An Alternative Schedule:
24hrs @ Room temp. 4hrs @ 40 Deg C 4hrs @ 50 Deg C 4hrs @ 60 Deg C 4hrs @ 80 Deg C
With regard to the PVC foam, as long as there is not significant pressure being applied to the core during heating you should not encounter any problems taking the core though to 80 Deg C, much beyond this and the structure of the foam may begin to deform and degrade.
Paul Statham Easy Composites / Carbon Mods - Technical
|