Hello ,
This is a great forum and I have gained immense knowledge here . Thank you guys !
After getting all supplies from easycomposites
I infused many carbon sheets on glass and a perfect glossy finish.
This is my first part I’m infusing in a mould.
Attempt 1 - pinholes towards the inlet side and relatively very less towards the vacuum side
( pinholes exactly between the fabric weave pattern )
It’s a 26”x 20” mould vacuum spiral was all around the flange of the mould and inlet in the center.
Mesh was right till the edge of the carbon fabric and spiral over the mesh.
This infused very fast approx 8-10 mins
Attempt 2 - pinholes all over the part. This time I infused from the side. Resin inlet spiral along the 26” side. I cut the mesh short and the spiral was over the peelply and carbon fabric. On the opp side I used two layers of the mesh on the flange and silicon connector in the middle.
This took about 20-25 mins to infuse.
Both times it was a perfectly sealed bag leak tested for 30 mins.
Where am I going wrong ? How do I get a pinhole free finish ?
Also which is the ideal way to place the inlet and vacuum on such a mould .
Really appreciate some help, thanks in advance


Replies
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Lester Populaire - 8/12/2020 3:08:17 PM
Just so everyone knows... DD compound is the manufacturer of the MTI hose that they praise here...

You say that like it's a bad thing. Dominik stands by his product, and so he should - it is a great product, there's nothing wrong with it. He also knows a lot about infusion, and I don't doubt at all that what he says is theoretically correct.

That said, and with all due respect to Dominik - I disagree that degassing is necessary, and I personally believe MTI Hose to be unnecessary as well. I would however absolutely recommend MTI Hose for beginners, it can really make the process simpler and more forgiving. I used to use it a lot, and I'll admit at the time I thought it was the bees knees and I got instant great results with it. These days, with more experience, I get those same results without the hose - hence it is not necessary to the process. For me, it became a high cost luxury product that wasn't really doing anything for me, and so I stopped using it. But if you are a hobbyist wanting perfect results and you're more concerned about the cost of wasting materials in a failed infusion than you are about paying a few extra $$$ for the hose, then it will probably help you.

Degassing - I find it causes more problems than it solves. As I said, theoretically I feel I agree with Dominik's understanding of the physics. It makes sense to degas the resin and further reduce the amount of air included in the infusion process. In reality though, I feel it just complicates the process. Not all resins are equal, some take longer to degas than others, and the whole time you are messing about with that your pot-life is ticking. All well and good if you are infusing a small component with 500g of resin and it will be done in 2 minutes, and it all fits nicely in a degassing chamber in one batch, but try messing about with degassing when you are infusing 15-20kg of resin. And considering I can get flawless pinhole free results without degassing, I again question it's necessity. 

End of the day, there's a lot of ways to skin a cat. Lots of people will find they get better results when they degas, lots of people will find they get better results when they use MTI hose, and power to them. We're all just trying to get perfect results, so whatever works for you is great. I offer my advice from my perspective, Mark can offer advice from his perspective, Dominik can offer his advice from his perspective, and hopefully between us we help some people nail an infusion!

Lester Populaire
L
Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)Supreme Being (2.9K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
Hanaldo - 8/13/2020 2:08:51 AM
Lester Populaire - 8/12/2020 3:08:17 PM
Just so everyone knows... DD compound is the manufacturer of the MTI hose that they praise here...

You say that like it's a bad thing. Dominik stands by his product, and so he should - it is a great product, there's nothing wrong with it. He also knows a lot about infusion, and I don't doubt at all that what he says is theoretically correct.

That said, and with all due respect to Dominik - I disagree that degassing is necessary, and I personally believe MTI Hose to be unnecessary as well. I would however absolutely recommend MTI Hose for beginners, it can really make the process simpler and more forgiving. I used to use it a lot, and I'll admit at the time I thought it was the bees knees and I got instant great results with it. These days, with more experience, I get those same results without the hose - hence it is not necessary to the process. For me, it became a high cost luxury product that wasn't really doing anything for me, and so I stopped using it. But if you are a hobbyist wanting perfect results and you're more concerned about the cost of wasting materials in a failed infusion than you are about paying a few extra $$$ for the hose, then it will probably help you.

Degassing - I find it causes more problems than it solves. As I said, theoretically I feel I agree with Dominik's understanding of the physics. It makes sense to degas the resin and further reduce the amount of air included in the infusion process. In reality though, I feel it just complicates the process. Not all resins are equal, some take longer to degas than others, and the whole time you are messing about with that your pot-life is ticking. All well and good if you are infusing a small component with 500g of resin and it will be done in 2 minutes, and it all fits nicely in a degassing chamber in one batch, but try messing about with degassing when you are infusing 15-20kg of resin. And considering I can get flawless pinhole free results without degassing, I again question it's necessity. 

End of the day, there's a lot of ways to skin a cat. Lots of people will find they get better results when they degas, lots of people will find they get better results when they use MTI hose, and power to them. We're all just trying to get perfect results, so whatever works for you is great. I offer my advice from my perspective, Mark can offer advice from his perspective, Dominik can offer his advice from his perspective, and hopefully between us we help some people nail an infusion!

I really like the MTI hose and we always have some in stock in the workshop. It can help a lot with complex shapes and moulds with a very small flange or things like that. back in the days i used it for pretty much everything and as you mentionned now it's more for special cases.

However i feel like degassing does help a lot depending on the fabric stack and flow rate it might be more or less important. We have it integrated in our workflow where it doesn't affect us too much and it is just nice for peace of mind where we know that this is one factor that we control and won't bite us.

i just think it is a little sleazy when the marketing department is praising there own product in an internet forum without stating how they are involved.

DD-Compound
DD-Compound
Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)Supreme Being (234 reputation)
Group: Forum Members
Posts: 25, Visits: 1.1K
I thought that the DD Compound in my signature is big enough 🤔
Also wrote several times here that DD-Compound is the producer.
I also agree to Hanaldo that the MTI hose is not a must. But the people how have enough knowledge and work on their own who get good results without tips and tricks is maybe 5%?
People who start or productions that need process stability are most of the composite users.
And also Hanaldo started one day and made his first successful infusions with my help and MTI 😉.
I am proud that he got that much knowledge and understood the process that he knows when he has to do what is necessary. When to degass and when not, using MTI or not, maybe reduce vacuum or not......
As simple as it is it is quite complex at the end of the day.
I am not making any money from smaller customers, usually we send also nice samples to all over the world to help beginners.
My reason to spread knowledge and help do more People understand the physics.
In the infusion industry is so much wrong information going around and also lots of „experts“ have no Clou what they do.
The tips I give here are to help people, and if they are followed you will get a perfect result.
I think it does not help if people just say this and that is not necessary but don’t explain why or just give that info for the special case.
I want to give people a toolbox so they are successful and understand the process. If they do that for a while they will understand more and more when what to do and of course if they are a pro they don’t need everything.
But you will see that if you for example have a big production things are more focused on process stability than on saving in materials.
I do infusions from 100g to 6tons of resin, the physics is the same but lots of parameters change. To much to explain everything so I always try to explain a process that works for 90%.

http://www.talkcomposites.com/Uploads/Images/f1d078f0-feab-4db2-8f2f-f009.png
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Xtreme - 5 Years Ago
Xtreme - 5 Years Ago
MarkMK - 5 Years Ago
Xtreme - 5 Years Ago
mscomposites - 5 Years Ago
Hanaldo - 5 Years Ago
mscomposites - 5 Years Ago
Perro007 gmail - 5 Years Ago
MarkMK - 5 Years Ago
DD-Compound - 5 Years Ago
Hanaldo - 5 Years Ago
Xtreme - 5 Years Ago
SleepingAwake - 5 Years Ago
Hanaldo - 5 Years Ago
SleepingAwake - 5 Years Ago
DD-Compound - 5 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search