Hi
I’m having issues with an imprint being left on my moulds and a little on the surface of my parts after I’ve infused the carbon.
Moulds were made using uni mould system, 5 layers of wax used for release, 1st layer of carbon is the pro finish. I have used a light spray of fusion fix, sprayed into the cloth before placing in the mould. Moulds have not been post cured
Just wondering if anyone had any ideas, my moulds now look like carbon print and to remove I’m having to 2000grit sams then polish, and my part has a slight dull finish on it but not all over but just sort of fibre in one direction, sorry not the easiest thing to describe and I tried to upload a pic but it’s not letting me upload
Any ideas
Cheers
Replies
emkayvr6
emkayvr6
Forum Guru (58 reputation)Forum Guru (58 reputation)Forum Guru (58 reputation)Forum Guru (58 reputation)Forum Guru (58 reputation)Forum Guru (58 reputation)Forum Guru (58 reputation)Forum Guru (58 reputation)Forum Guru (58 reputation)
Group: Forum Members
Posts: 5, Visits: 20
Ok thanks warren, will take those points into consideration in future 👍
Was using a mix of slow and fast hardner, may have been a little green when I demoulded, Had been 18hours but prob only 18-20 degrees, will give it a bit longer next time.
Thanks
beliblisk
b
Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)
Group: Forum Members
Posts: 53, Visits: 2.8K
emkayvr6 - 6/18/2020 9:26:57 AM
Ok thanks warren, will take those points into consideration in future 👍Was using a mix of slow and fast hardner, may have been a little green when I demoulded, Had been 18hours but prob only 18-20 degrees, will give it a bit longer next time.Thanks

I normally leave parts in for solid 48h or more. 

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
emkayvr6 - 5 Years Ago
taimur - 5 Years Ago
beliblisk - 5 Years Ago
emkayvr6 - 5 Years Ago
beliblisk - 5 Years Ago
emkayvr6 - 5 Years Ago
Warren (Staff) - 5 Years Ago
emkayvr6 - 5 Years Ago
                 I normally leave parts in for solid 48h or more.
beliblisk - 5 Years Ago
okkim - 5 Years Ago
Hanaldo - 5 Years Ago
okkim - 5 Years Ago
Hanaldo - 5 Years Ago
okkim - 5 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search