That doesn't look too bad for a first hit at all!!
Could be a few issues like minor air leak, infusing too quick, leaving pump running with inadequate resin barrier, etc. The corners look good so I suspect very little if any bridging which is good for such a complex shape.
In essence you may just need a bit more resin in the laminate. If you leave the resin feed open for an extra 30 seconds to a minute after clamping the vacuum line then you should have plenty of resin in the part.