Making a Large high temp curing oven


Author
Message
Kairu
K
Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)Forum Guru (68 reputation)
Group: Forum Members
Posts: 7, Visits: 13
Without spending an obscene amount of money for an oven is it possible to create one large enough for like a 16’ boat hull with high temps ranging 250-300 f?

If so what kind of things do I need? This area is not something I’m intimately familiar with.
Replies
Chris Rogers
C
Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)
Group: Forum Members
Posts: 120, Visits: 933
I agree with everybody here.  SSR and PID controllers are great.  Circulating fans are key.  Fire-proof insides are a good idea.  It's still dangerous and you really have to be careful that stuff can't get sucked into the heaters.  And 120C is pushing the upper end of what is comfortable for a home-made oven...  I don't really see the advantage of curing low-temp pre-pregs above 90-100C given how hard it can be on tooling, CTE issues and problems with foam cores.  There are lots of good resin systems that work beautifully in this range.

Here's a post on making and buying ovens:  https://explorecomposites.com/articles/tools-and-equipment/oven-options-for-pre-preg-curing/

But really, be careful!  I have had oven heater fires (and close calls) and they're scary!




beliblisk
b
Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)
Group: Forum Members
Posts: 53, Visits: 2.8K
I did simple 4x4cm metal frame, insulated with 5cm alu sided panels, heated by 2kw industrial blow heater and cover everything with 25mm wood boards.......still runing cheap ebay PID controler trought SSR as i was only using it for infusion post cures (60 deg).

Dimensions are 200x100x90

Next step will be Omega PID and perhaps one more heating/blowing element if needed (tho i plan to use low cure cycle for prepegs).


Steve Broad
Steve Broad
Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)Supreme Being (3.4K reputation)
Group: Forum Members
Posts: 408, Visits: 4.1K
Chris Rogers - 5/14/2020 4:52:35 PM
I agree with everybody here.  SSR and PID controllers are great.  Circulating fans are key.  Fire-proof insides are a good idea.  It's still dangerous and you really have to be careful that stuff can't get sucked into the heaters.  And 120C is pushing the upper end of what is comfortable for a home-made oven...  I don't really see the advantage of curing low-temp pre-pregs above 90-100C given how hard it can be on tooling, CTE issues and problems with foam cores.  There are lots of good resin systems that work beautifully in this range.

Here's a post on making and buying ovens:  https://explorecomposites.com/articles/tools-and-equipment/oven-options-for-pre-preg-curing/

But really, be careful!  I have had oven heater fires (and close calls) and they're scary!

The main advantage of going to 120 deg C is the time factor. One hour at 120 or 4 hours at 100 or 8 hours at 90. I find 120 works fine and have had no issues......so far :-) I had to go down to 80 deg for one cure cycle as I had used a standard mould putty instead of a high temp one. 16 hours!

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Kairu - 5 Years Ago
Steve Broad - 5 Years Ago
Kairu - 5 Years Ago
Steve Broad - 5 Years Ago
Hanaldo - 5 Years Ago
Kairu - 5 Years Ago
Steve Broad - 5 Years Ago
explorecomposites - 5 Years Ago
beliblisk - 5 Years Ago
Steve Broad - 5 Years Ago
scottracing - 5 Years Ago
Kairu - 5 Years Ago
Steve Broad - 5 Years Ago
Hanaldo - 5 Years Ago
Steve Broad - 5 Years Ago
Kairu - 5 Years Ago
Hanaldo - 5 Years Ago