Hi guys,
I’m new to resin infusion, I finally made a sealed mould and did a drop test before infusing.
I did a 3h drop test in which it held vacuum pressure.
The ambient temp was between 25-30 degrees Celsius.

The resin was de gassed
I started infusion by slowly loosening the hose clamp on the resin side while the pump was running.
Once I got full wetout, I clamped the vacuum side, and about 30s later I clamped the resin side.

everything looked fine for 2 minutes, then I started noticing the bubbles within the flow media, these bubbles started forming in different areas of the part.

Then I noticed some areas of the bag were very loose, e.g the area where the vac hose connects to the bag.

I’m not sure what’s causing this but it’s the second time it’s happened to me!

Would appreciate some help Smile

Thanks
Reply
8900120d
8900120d
Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)Supreme Being (308 reputation)
Group: Forum Members
Posts: 37, Visits: 939
MarkMK - 6/18/2019 6:16:05 AM
It can sometimes happen that a leak occurs after the part has infused, even where vacuum was securely held prior to and during infusion. Sometimes the effect of resin running through the part can loosen some part of the perimeter tape and it can become more prone to happening where the bag is quite tightly held

Looking at your picture, it does look like your pleats were quite small and, perhaps, there was some excessive strain around these areas, even though the part looks quite small

I'd recommend using slightly bigger pleats and trying to position the bag so that there's the minimum of strain on them whilst pulling down the vacuum. A bag with plenty of slack will produce less strain on the perimeter tape and it's also worth going around the entire perimeter and pressing things down firmly juts prior to infusion, even if it appears that full vacuum is achieved, just for added certainty

Make sure also that you wipe the areas where the tape is placed to make sure that there's not a build-up of release agent there that might make the tape a bit less sticky when applied. Observe the part for a few minutes after infusion and try to press the tape down quickly if you notice any 'creep' of air occurring, which might help stop the whole part being compromised

Careful prep of the bag should, hopefully, limit the occurrence of such issues, but it can sometimes happen quite inexplicably. On a flat-ish mould, with very clean flange areas, it should be quite rare, though


Thanks for your reply Smile 
i also have another mould which i envolope bagged, i didnt have to use any pleats as the mould was quite flat, but i had the same issue. could it be due to the resin exotherm? 
 slow hardener and 5min degassing.

Edited 6 Years Ago by 8900120d
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
8900120d - 6 Years Ago
8900120d - 6 Years Ago
MarkMK - 6 Years Ago
8900120d - 6 Years Ago
Warren (Staff) - 6 Years Ago
8900120d - 6 Years Ago
Warren (Staff) - 6 Years Ago
MarkMK - 6 Years Ago
Michael Stuart - 6 Years Ago
MarkMK - 6 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search