Glasscast 10 pouring resins are easy ways to eliminate bubbles


Author
Message
Asurada
Asurada
Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)
Group: Forum Members
Posts: 10, Visits: 954
Hello everyone, I recently made some things with glasscast10 resin, I want to make 0 bubbles of transparent resin parts. In the use of found a very troublesome thing, glasscast10 in the mixing, it is difficult to eliminate the bubbles in the resin, I used the vacuum degassing and hot air gun heating way to eliminate bubbles, but it is difficult to eliminate the bubbles in the resin. At first I thought the vacuum degasification way is the most ideal way to eliminate bubbles, but glasscast10 in the vacuum degasification process, there will be a lot of small bubbles, more than the appearance of non-degasification bubbles, this is what reason? The following photo is a workpiece I just made out of a degasification method.Hello everyone, I recently made some things with glasscast10 resin, I want to make 0 bubbles of transparent resin parts. In the use of found a very troublesome thing, glasscast10 in the mixing, it is difficult to eliminate the bubbles in the resin, I used the vacuum degassing and hot air gun heating way to eliminate bubbles, but it is difficult to eliminate the bubbles in the resin. At first I thought the vacuum degasification way is the most ideal way to eliminate bubbles, but glasscast10 in the vacuum degasification process, there will be a lot of small bubbles, more than the appearance of non-degasification bubbles, this is what reason?

Thickness:20mm
Then I tried vacuum degassing and hot air gun two methods together to defoaming, but I probably use hot air gun repeatedly to blow to the heating used four or five times to be able, basically I recognize the bubble elimination of almost, with the hand touch silicone mold will feel the resin has become hot, in a period of time the resin has begun to gel. It's ideal to do this, but there are still a few bubbles. Shown in the following figure.

Thickness:30mm

Replies
oekmont
oekmont
Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)Supreme Being (4.8K reputation)
Group: Forum Members
Posts: 550, Visits: 27K
It seems to me that your are working in too cold conditions. The diamond looks clear on the surface where you heated the resin. The room temperature should be 25°C and the resin should keept at this temperature at least several hours before mixing.

Asurada
Asurada
Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)Supreme Being (93 reputation)
Group: Forum Members
Posts: 10, Visits: 954
oekmont - 4/18/2019 10:12:30 AM
It seems to me that your are working in too cold conditions. The diamond looks clear on the surface where you heated the resin. The room temperature should be 25°C and the resin should keept at this temperature at least several hours before mixing.

Is it heavily affected by temperature? I am using the resin in 35 ℃ environment insulation 1 one hours after the use, but the curing and operation of the ambient temperature will be above 15 degrees Celsius

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Asurada - 6 Years Ago
Asurada - 6 Years Ago
Tom (Staff) - 6 Years Ago
             Glasscast 10
Asurada - 6 Years Ago
oekmont - 6 Years Ago
Asurada - 6 Years Ago
oekmont - 6 Years Ago
JasonFL - 6 Years Ago
Rich (Staff) - 6 Years Ago