Just tried my first flat sheet 195g 2x2 c/f, and failed. I am using a polished aluminium table 2.4  x 1.7 Metres, No 8 wax, No 2 resin. I want a single thickness for decoration only. I waxed the Ali sheet and then tried to coat with epoxy, it kept producing pinholes which quickly opened up to bare circles the size of a penny. I brushed it over several times and gradually reduced the number of void circles but clouded the resin here and there, I assume with wax. I did press on and finish the sheet with Vac but had a persistent very slow leak, I just re pumped every 20 mins for 3 hours. The finished sheet (1/2mm thick) also shows tiny voids where the weave crosses. Perhaps I made some schoolboy errors here but a few hints would be much valued. I am wondering if everything was too cold at 12 deg?
Reply
prairiecustomcomposites
prairiecustomcomposites
Supreme Being (184 reputation)Supreme Being (184 reputation)Supreme Being (184 reputation)Supreme Being (184 reputation)Supreme Being (184 reputation)Supreme Being (184 reputation)Supreme Being (184 reputation)Supreme Being (184 reputation)Supreme Being (184 reputation)
Group: Forum Members
Posts: 26, Visits: 722
This isn't the first time I have heard of wax creating voids and spots where epoxy simply will not go. Did you have any clumps or small "hills" of wax sitting on the surface of the aluminum? Or did you buff it all off? It sounds to me like there was too much wax left on the aluminum. If you can post some pictures of the carbon piece that came out that would be great.

As far as the temperature goes, 12 degrees Celsius is pretty cold for epoxy. I believe for most epoxies you normally want no less than 22 degrees. The lower the temperature, the higher the viscosity (thicker) it will be, which usually entraps bubbles, but in your case, it sounds like they are not the usual bubbles that every epoxy user tries to fight off. That being said, 12 degrees seems cold enough that I would think the epoxy would take forever to actually cure.

It could also be an incompatibility between the brand of resin and brand of wax - maybe they slightly attack each other? I saw on a forum once to be sure the mould release wax is a pure carnauba wax (which I assume all mould release waxes are). Hope this helps.

-Mike-
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search