Hi Guys, 

Use for bonding carbon fiber with carbon fiber or metal based adhesive Methyl Methacrylate however is missing from my suppliers.
I don't buy Vudu Glu because i live in South America.

What can I use to replace vudu glu (adhesive Methyl Methacrylate) ?
Hanaldo
Hanaldo
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Epoxy will be the best alternative. 
Dezer
Dezer
Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)
Group: Forum Members
Posts: 74, Visits: 1.8K
[citar]
[b] Hanaldo - 8/14/2018 2:34:46 AM [/ b]
Epóxi será a melhor alternativa. 
[/ citar]

Blend of epoxy with fumed Silica (Aerosil) is it a good solution?
What proportion aerosil x epoxy use?



Hanaldo
Hanaldo
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Dezer - 8/14/2018 3:39:29 AM
[citar]
[b] Hanaldo - 8/14/2018 2:34:46 AM [/ b]
Epóxi será a melhor alternativa. 
[/ citar]

Blend of epoxy with fumed Silica (Aerosil) is it a good solution?
What proportion aerosil x epoxy use?



Depends on the application. It will do a decent job in most cases, but for anything critical I would be using a proper toughened structural epoxy adhesive.

How much to add depends how thick an adhesive you want and how thick your base resin is to begin with. For something like a paste adhesive, you will probably want to start at 5% and then go from there. I'd also recommend adding some cotton flock as well.


Edited 8 Years Ago by Hanaldo
Dezer
Dezer
Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)Supreme Being (712 reputation)
Group: Forum Members
Posts: 74, Visits: 1.8K
Hanaldo - 8/14/2018 4:43:53 AM
[quote]
Dezer - 8/14/2018 3:39:29 AM
[citar]
[b] Hanaldo - 8/14/2018 2:34:46 AM [/ b]
Epóxi será a melhor alternativa. 
[/ citar]

Blend of epoxy with fumed Silica (Aerosil) is it a good solution?
What proportion aerosil x epoxy use?



Depende da aplicação. Ele fará um trabalho decente na maioria dos casos, mas para qualquer coisa crítica eu estaria usando um adesivo epóxi estrutural endurecido adequado.

Quanto a adicionar depende de quão grosso um adesivo você quer e quão espessa sua resina básica é para começar. Para algo como um colar adesivo, você provavelmente vai querer começar em 5% e depois ir a partir daí. Eu também recomendo adicionar algum lote de algodão também.

[/citar]

The application are automotive accessories.
Does the Epoxy + Aerosil blend work well for this application?