Hello all,

              I am currently having a problem with my Xpreg XC110 prepreg. In my last test the prepreg did not cure and was still  gooey once the cure cycle was complete. My oven, which is home is set up with a proper PID controller complete with the thermo coupling. Its shows to have reached the temperatures that are recommended for the XC110 system. My mold is a CNC'ed piece of aluminum 2" thick. The mold itself is 20" x 46" x 2" With basically the back and sides of a guitar cnc'ed into it. When I did the trial run once it had soaked for an hour at the higher temp I lifted the oven off the mold so it could room cool. So, what would be my problem? 
A. I should have left the oven over the part to let it slow cool
B. the aluminum is taking to long to reach temperature
C. the oven isn't actually reaching the temperature the thermo coupling says it is. 
Any other ideas on what it may be would be of great help.

Also, unlike the video my surface finish is almost like dry carbon, there is no clear looking finish on it at all. Does the Paper side of the pre-preg go down first or the plastic side? or does it matter? and could it be the either over cooked or under cooked problem that could have also caused that?  Any help would be greatly appreciated. Thanks!

JC
Replies
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Placing thermocouples in direct contact with an aluminium mould can also cause trouble though, as the PID thinks the oven isn't heating up and so it tries to crank the heat as fast is it can. This heats the air up to extreme temperatures, so you can lose control of your ramp rates and your soak temp.
Fasta
Fasta
Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)Supreme Being (4K reputation)
Group: Forum Members
Posts: 468, Visits: 3.5K
Hanaldo - 6/22/2018 12:19:04 AM
Placing thermocouples in direct contact with an aluminium mould can also cause trouble though, as the PID thinks the oven isn't heating up and so it tries to crank the heat as fast is it can. This heats the air up to extreme temperatures, so you can lose control of your ramp rates and your soak temp.

This is the exact reason I read from the air with a heavy metal mould. I also cook multiple parts/moulds of different sizes in the each cooking session. When oven goes crazy trying to heat a metal mould at 2 deg per min the heat from the elements just run flat out can fry the other parts a bit with near burnt bags from the radiant heat. Just adding an extra hour to the cure time means that all the parts get enough and work out.

In the end all that matters is that a part gets it correct cure temp for at least the minimum time.





Jeff Clemmons
J
Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)Forum Guru (61 reputation)
Group: Forum Members
Posts: 6, Visits: 45
So what I have done is drilled holes up through the bottom of the mould which are 1 1/2" deep in  2" mould. My plan is to run the mould empty through a cycle and testing various places in the mould as it heats. Once I see that the entire mould is up to temp, I will add that amount of time to the "soak" time. That way my air inside the mould isn't ramping to quick and I will know everything is leveled of at the correct soak temp. I plan on running this test this weekend. Thank for the comments guys!

JC
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Clemm - 7 Years Ago
Fasta - 7 Years Ago
nreindel - 7 Years Ago
Hanaldo - 7 Years Ago
Warren (Staff) - 7 Years Ago
Clemm - 7 Years Ago
Hanaldo - 7 Years Ago
Warren (Staff) - 7 Years Ago
Clemm - 7 Years Ago
Warren (Staff) - 7 Years Ago
MarkMK - 7 Years Ago
Clemm - 7 Years Ago
Hanaldo - 7 Years Ago
Fasta - 7 Years Ago
Clemm - 7 Years Ago
f1rob - 7 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search