Hello friends,

I intend to make a medium-sized piece (1.35mx 0.30m) with polyester resin, but I saw that it corrodes the potential risk of shrinkage during resin curing.

- The resin has the gel time of: 30 minutes and the manufacturing process would be by Hand Layup + vacuum bag or Resin nfusion.

The doubts are as follows:

"What do I have to do to stop this from slowing down?"
Because I can not have dimensional changes due to the product accessories.

Desmoulding after 4 hours of lamination cause me problems?

We have a small production line and we need to be quick in our process.

Thanks,
Dezer

Edited 7 Years Ago by Dezer
Reply
ana
a
ana
posted 5 Years Ago HOT
Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)Supreme Being (188 reputation)
Group: Forum Members
Posts: 14, Visits: 49
oekmont - 2/19/2018 7:30:03 AM
no, I am talking about the first hour of curing. polyester reaches this "jelly stage" in wich it is no longer liquid, and cannot flow infinitely under shear stresses (the definition of a liquid). from this point on, the resin still shrinks massively, but cannot flow anymore, to compensate the shrinkage.
and I not talking about my experiences, this is state of the art university knowledge. you can find this information in "konstruieren mit faser-kunstoff-verbunden" written by Helmut schürmann, professor at TU Darmstadt. one of the best (mostly theoretical) books about composites in my opinion.

I forgot a good countermeasure against warping and shrinking:
use woven cloth instead of chopped strand mat. and use a symmetrical layup. for example layer a, then layer b, then b and finally a again.
with woven cloths you can achieve higher fibre contents, and the symmetrical layup cancels the warping forces out against each other.

Hi my friend 
Please help me
I apply gel coat as first layer . After 2 hrs I apply second layer " mixed polyester resin  around 35% and 5 % pigment and silica powder 30 % and carbonate calcium 30 % as filler around 60 %
I demold after 1 hrs but back side of mold comes out very good but top side is not come out easily .
Please help me what is my problem ?
Also I add cobalt 0.05 % and peroxide 1.8 %
How can i remove my part easily  ?
My part thickness is 1.2 mm

Tanks so much in advance
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
Dezer - 7 Years Ago
Hanaldo - 7 Years Ago
oekmont - 7 Years Ago
Hanaldo - 7 Years Ago
oekmont - 7 Years Ago
ana - 5 Years Ago
Warren (Staff) - 5 Years Ago
ana - 5 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search