Epoxy pot life


Author
Message
andy47
a
Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)
Group: Forum Members
Posts: 22, Visits: 95
I have a low viscosity epoxy + hardener with a 150-minute pot life. However, the epoxy that's mixed in a cup starts warming up in 30 minutes and hardens in one hour while producing a lot of heat. The epoxy that's infused in the part hardens in a few hours which is correct. This is not an issue for small projects where the epoxy is infused in less than an hour, but I am worried what if the infusion process takes longer. How do you deal with this issue - the epoxy warming up in the cup which results in a much shorter pot life than stated?

Reply
andy47
a
Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)
Group: Forum Members
Posts: 22, Visits: 95
Hanaldo - 11/18/2017 9:58:51 PM
andy47 - 11/18/2017 3:25:44 PM
I have a low viscosity epoxy + hardener with a 150-minute pot life. However, the epoxy that's mixed in a cup starts warming up in 30 minutes and hardens in one hour while producing a lot of heat. The epoxy that's infused in the part hardens in a few hours which is correct. This is not an issue for small projects where the epoxy is infused in less than an hour, but I am worried what if the infusion process takes longer. How do you deal with this issue - the epoxy warming up in the cup which results in a much shorter pot life than stated?

The 150 minute pot-life will be for a given mass, usually 100g or 500g (it should specify on the data sheet). 

If you're mixing more than that then it will significantly shorten the pot-life, as you've experienced. The only real solution for doing large quantities is to mix several smaller batches. I never mix more than 1kg at once, but have the rest measured out and ready to mix as soon as the infusion starts. 

I have been thinking about this, but how do you change the cups during the infusion process? I am worried that if I pull the hose out of the cup, a bubble will get inside even if I close the clamp.