Hi All, 

I have tried to find some info on here but possibly did not use the same search terms so please excuse me if this has been repeated.

I have made some CF panels on a glass sheet  using 2 x 200gm² sheets pressed together. In one case i have used peel ply on the reverse to clear excess resin.


I have noted that these parts and panel came out soft and flexible.  It also has a slight wrinkled surface when folded or flexed.

The flexibility can be compared to that of a common computer mousepad.



Anyone had this happen or have an explanation ?


The only reason I can possible think of is ambient temperature, I remember the days where pretty cold and humid during and my workshop is an open space.

I have also let the parts rest for a few says hoping that they would cure and harden a little... but no luck.

Seems like this panel and other parts I made during those days have all come out the same way...   Blink

http://www.talkcomposites.com/Uploads/Images/ede72a04-6225-42a7-8273-54e6.JPG 
Fasta
Fasta
Supreme Being (6.6K reputation)Supreme Being (6.6K reputation)Supreme Being (6.6K reputation)Supreme Being (6.6K reputation)Supreme Being (6.6K reputation)Supreme Being (6.6K reputation)Supreme Being (6.6K reputation)Supreme Being (6.6K reputation)Supreme Being (6.6K reputation)
Group: Forum Members
Posts: 468, Visits: 3.5K
I reckon this must be a resin mixing error or just too cold to cure??




Dravis
Dravis
Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)Supreme Being (8.6K reputation)
Group: Forum Members
Posts: 592, Visits: 1.9K
A combination of even slightly off mixing ratio and too low temperatures could be the problem.

Some resin systems are very critical in relation to mixing ratios -- I did a few tests with EC IN2 -- you need to be within 5-10% of the correct weight. This is almost impossible to do on small batches (Less than 50 grams)

IN2 will not harden properly if temperatures are below 16-18 degrees Celcius, even if correctly mixed, they will absorb a lot of moisture in humid conditions, making the resin soft.

"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Definitely a cure issue of some kind.  That is almost as flexible as a sheet made with our EF80 flexible resin!

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Rich (Staff)
Rich (Staff)
Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)Supreme Being (2.3K reputation)
Group: Administrators
Posts: 167, Visits: 4.6K
A couple of questions to help us understand and hopefully advise accordingly: 1)Were these wet laid? 2) What resin did you use?
fibernoob
fibernoob
Supreme Being (662 reputation)Supreme Being (662 reputation)Supreme Being (662 reputation)Supreme Being (662 reputation)Supreme Being (662 reputation)Supreme Being (662 reputation)Supreme Being (662 reputation)Supreme Being (662 reputation)Supreme Being (662 reputation)
Group: Forum Members
Posts: 34, Visits: 134
Hey all....  After reading the replies, remembering what happened and calling the suppliers ... I found out what went wrong w00t

I had purchased  lower viscosity resin thinking that it would produce less air bubbles during the vacuum process.

ExclamationIt occurs that this resin has a slightly different mixing ratio and is more sensitive to temperature. Exclamation


Thanks again for all the helpful input from everyone, nice to see how accurate all the answers are.