We are trying to create carbon wing (see photos) from textrem with infusion, almost whole wing is ok, but last part, after few minutes on sun it goes wrong.

Can you please give us some hint, what we are doing wrong?

http://www.talkcomposites.com/Uploads/Images/1d26313f-08d3-4bcf-893a-f4e1.jpg
http://www.talkcomposites.com/Uploads/Images/45602c20-0b14-42f2-9d23-44b4.jpg
Replies
carbonfibreworks
carbonfibreworks
Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
Hi
What type of resin are you using ? are you allowing enough time before you de mould and have you post cured the part ?
Chris
Carbon fibre works LTD

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
chosecz
chosecz
Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)
Group: Forum Members
Posts: 2, Visits: 8
We are using resin ATLAC 590 (CAS-100-42-5). Yes, we are allowing enough time before de mould. No, we didn't do any post cure.

Another example - from begining is ok, but end is really bad.

http://www.talkcomposites.com/Uploads/Images/7650fb28-663b-41e4-901c-8e30.JPG
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search