Hello wonder if any one can help me with a few problems I'm having.

A. I've Carbon laminated a motorbike petrol tank with B & R carbon, my problem is that I cant seem to get rid of the grey water marks or small little dots. Tried using acetone & ethanol, tried polishing, I just cant get rid of them, I'm hesitant to sand much more because in places its starting to break through and the satin isn't as robust as the carbon.

B. I've resin laminated the whole frame, however when I'm trying to get a polish finish using wet and dry little white dots start showing up like they are in the resin it self.
I did used flumed silica to give the base layer a decent ability to hold, but I left it a long time with the black colouring paste as suggested.

I also use my catch pot chamber as a vacuum chamber to take out as much of the air as I could.

This is my first attempt at a composite project so am a little unsure. tbh I'm getting a little frustrated with it now, I just want my bike back in one piece, the amount of hours I have put in is getting ridiculous.

Any help would be much appreciated

Joel
Reply
Dravis
Dravis
Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)Supreme Being (5.1K reputation)
Group: Forum Members
Posts: 592, Visits: 1.9K
Seems like several things went wrong here...

The Tank image, shows what looks to me like delamination between layers of top-coat epoxy (Coating Epoxy?)   Did you wet sand and degrease between coatings of Epoxy?

Also did you work at low temperatures or in high moisture environment ? That may explain the "cloudy" areas.  If they are only in the top coatings, they can probably be sanded away.

The little white dots are "pinholes" from very small airbubbles in the resin... Very hard to get rid of completely, which is why I often wet sand, and do a 2-component clear coat on "skinned" parts.
That makes most of the pinholes invisible or nearly so.

With great care you may be able to wet sand down to just above the Carbon fibres, and then clear-coat.  That may save your work.  If you do sand into the weave, it will give that area a slightly different look.
I've done a few parts where I sanded the whole part down into the weave, and by doing it carefully and evenly, it can come out looking very nice anyway, but a real Carbon "geek" will spot it  ... BigGrin

"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...





Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search