Preface: This is the first time I've ever touched fiberglass, resin or even CF

Excuses: I'm a noob Wink  Working outdoors (under cover though)  It's winter here so temps and conditions (very windy) aren't ideal.  Etc... Tongue

Products: Vinylester tooling gel coat, polyester resin + 198 cloth, wax + PVA

Attempt #1: Mixed up tooling coat + hardener using incorrect ratios.  Scrapped first attempt and started over.

Attempt #2:  I'm attempting to make a mold of my engine cover as it seems like a fairly simple part to start with.  As you can see from the pic, I raised the part off my polycarbonate sheet slightly and then plugged up the bolt holes with filleting wax as well as smoothly extending/blending the sides of the part onto the base with some more wax.



I then applied 6 layers of mold release wax to the part as per the manufacturers instructions.  Followed by a single layer of PVA applied by brush, again, as per manufacturer instructions.  I do not currently have access to any spray equipment.

Stupidly I didn't apply any wax or PVA to the polycabonate sheet underneath as I though nothing would stick to it.  Doh!

Next, I mixed up the tooling coat (@1.5%) and applied it to the part and base as pictured.



I left it overnight (perhaps a little too long) till it was tacky.  I mixed up the polyester resin (again @ 1.5%) and applied it to the tooling coat.  I then started off with one layer of 198 FG cloth.  However, I could see issues starting to develop already so at that stage I made the decision that I wasn't going waste any more product and I was going to finish off the mold "as is" and use it as a learning experience.



I had pre-cut the cloth as one large piece in the hope that it would drape over the part easily and conform.  However, because of the indentations for the bolt holes, every time I tried to push it into place it would pull and lift elsewhere creating air voids.  I tried to roll the air out but to no avail.  Next time I will pre-cut the cloth differently, or alternatively, I plan on using CSM instead of cloth which looks like it might be more conformable.



So, I only applied 2 layers of cloth as best as I could, knowing full well that it was not going to cut it, and left it at that to cure for the next few days.

Today I pulled the mold apart and as could be expected, it wasn't pretty Smile



However, once I had the mold separated from the base, my part almost fell out of the mold without any effort so it seems that at the very least my waxing and PVA efforts worked.

In any case, I have some observations and some questions I'm hoping you guys could help me with.

Looking at the below pic, does my tooling coat look thick enough?



Should I have applied a second tooling coat once the first coat went tacky?

I probably let the tooling coat set too much (it was still very slightly tacky but not what I expected) before applying the FG cloth as it looks like the bond between the tooling coat and FG isn't very good.  Would I be correct in my assumption?  Generally, how long should I wait for a tooling coat to start to set?

I'm also not happy with the finish of the mold surface from the PVA.  I've tried finding Frekote/EasyLease/Chemlease locally but it's like hens teeth over here Sad  Would applying the PVA in multiple coats and or with a sponge give a better result/finish?



Thank you in advance for reading my short novel. Wow

I'll be attacking this mold again as soon as I've re-evaluated my process so any constructive criticism and or advice you guys can provide a noob would be very much appreciated.

Cheers,



Edited 11 Years Ago by BoostSamurai
Reply
remodovakhin
remodovakhin
Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)Junior Member (14 reputation)
Group: Forum Members
Posts: 2, Visits: 14
Hi guys! I am a noob and newbie in Fibreglass stuff. I am a fourth year engineering student actually. We are making the body of our car for the Shell Eco Marathon actually. This is also our first time. the plan is to first build a plug and then make a female mould using fibreglass and then applying carbin fibre on the insides on this mould to get the final carbon fibre car body. SO we have bought a few fibreglassing items:-

I have purchased pre-accelerated Vinylester Resin Crystic VE679 PA, pre-accelerated Polyester Resin Crystic RTR 4000PA, Crystic GelCoat 12 PA Pine Green, Surface Primer Grey Nord 210 lAQUE, Surface primer Nord 230, methylene Chloride (like acetone) and 450g/m2 CSM glass matt. I also have the catalyst MEPOXE. Now my problem is i am a little confused about these chemicals. I want to build a fibreglass female mould using these chemicals. So firstly we are planning to build a plug using mdf and pour foam. Then the plan is to apply putty or body filler to fill in pores and gaps on the plug surface, this will then be sanded. Then i would apply 'Mould kanstik sealer' to seal porosities. Then next i would apply the gelcoat, followed by ... I am lost then. Can someone here please guide me on how i can use the above chemicals to build my plug to good smoothness and then create my female fibreglass mould. i cannot thank you enough for your help! 

Also some of my questions are-  Do the Vinylester and the Polyester resins mentioned above require a hardener chemical as well to cure or is it just enough to add the catalyst? And how much catalyst am i to add normally? Also what is the difference between the Vinylester resin and the polyester resin? Are these chemicals used together or do i just use one of them to put on the fibreglass? 

Your answers are highly appreciated!

Thanks and Regards
Hoping to hear from you PROS soon!
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
BoostSamurai - 11 Years Ago
BoostSamurai - 11 Years Ago
winty - 11 Years Ago
Hanaldo - 11 Years Ago
BoostSamurai - 11 Years Ago
Hanaldo - 11 Years Ago
George Sychrovsky - 11 Years Ago
ajb100 - 11 Years Ago
kidpaint - 11 Years Ago
BoostSamurai - 11 Years Ago
remodovakhin - 11 Years Ago
Dravis - 11 Years Ago
remodovakhin - 11 Years Ago
ajb100 - 11 Years Ago
Hanaldo - 11 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search