TomDesign
TomDesign
posted 11 Years Ago
ANSWER
HOT
Topic Details
Group: Forum Members
Posts: 454,
Visits: 2.5K
Guys i tryed my first infusion.
so i cleaned with mold cleaner then layed easylease
then all those thing to do infusion temperature was like plus 15 i made at 7 like pm and in the morning at 11 i went and still it was not dryed normally where is problem? temperature? as i mixed and put hardener perfectly! also i took it out and i saw like it had like empty places in pattern, i checked no leaks.
Please advice.
Reply
Like
3
TomDesign
TomDesign
posted 11 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 454,
Visits: 2.5K
by the way i tryed and clear gelcoat easycomposites why its acted like that you can see in couple spots not cured it was mixed good i think maybe to big layers i spread?
also why this think that has to show leak never turns when it leak?
Reply
Like
2
Hanaldo
Hanaldo
posted 11 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 2.5K,
Visits: 28K
Looks like your gelcoat was too thin.
I don't find those flow indicators very useful for finding leaks at all, certainly not any that you can't hear anyway. I do however find it quite useful for determining when the air has been completely evacuated, as mine always spin for a fair time after the bag has pulled completely tight.
Reply
Like
3
TomDesign
TomDesign
posted 11 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 454,
Visits: 2.5K
and what about curing problem that wrote?
Reply
Like
2
Hanaldo
Hanaldo
posted 11 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 2.5K,
Visits: 28K
My suspicion would certainly be temperature. I would be letting it cure for 24 hours at 25 degrees, if you're at 15 degrees I think you need to either heat it up a bit (best solution) or just leave it longer (48-72 hours). You could try post-curing it in an oven now that you've already demoulded.
Reply
Like
2
Matthieu Libeert
Matthieu Libeert
posted 11 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 955,
Visits: 3.4K
15°C is not enough of temperature to make composites in a good way... I would never start working on a project when my room temperatures are under 20°C
Like Hanaldo says it would need to cure for more than 2 days before demoulding. Even at 25°C I wait 2 days
Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com
Reply
Like
3
TomDesign
TomDesign
posted 11 Years Ago
ANSWER
HOT
Post Details
Group: Forum Members
Posts: 454,
Visits: 2.5K
ouu thanxs guy. also any ide on gelcoat? i think to thin layer?
Reply
Like
3
GO
Merge Selected
Merge into selected topic...
Merge into merge target...
Merge into a specific topic ID...
Open Merge
Post Reply
Like
3
Similar Topics
Post Quoted Reply
Reading This Topic
Login
Login
Remember Me
Reset Password
Resend Validation Email
Login
Facebook
Google
Explore
Messages
Mentions
Search