Just saw this thread, while scouting through old ones ... Yeahh Im Bored ....Whistling

The "damage you are seeing in the Carbon ends of the tubes looks VERY much like the resin has been damaged by too much UV light..

It would make sense, since the Aluminium has probably been polished many times, and the ends of the tubes have had a part of the protective clear coat worn away.

This is a death sentence for the CF tubes I'm afraid ... they will loose a significant part of their strength.

But ... all is not lost, just make new tubes for the nice joints ... should not be too hard a job, if they are round tubes, you can just buy them and reinforce them as needed..

... Good Luck....

"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
FLD
FLD
Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)Supreme Being (3.7K reputation)
Group: Forum Members
Posts: 468, Visits: 2.7K
Whilst galvanic corrosion is unlikely for this (no dissimilar metals) it is possible that water has gotten into the joints and the aluminium has corroded.  Aluminium oxide is something like ten times the size of aluminium.  This could essentially burst the carbon tubes which have very little give.  The marks come from the damage to the laminate.  I think its one of those ride at your own risk jobs I'm afraid. 
Edited 12 Years Ago by FLD
Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Its what you can't see that worries me!!

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
erikrhendrickson
erikrhendrickson
Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)
Group: Forum Members
Posts: 3, Visits: 3
No cracks or any other signs of wear along the tubes...just the ends near the lugs.
Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
does sound like moisture penetration and some nasty galvonic corrosion going on.

Problem is if the aluminium has expanded much then the tubes may well have serious structural cracks along thier length.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Edited 12 Years Ago by Warren (Staff)
carbonfibreworks
carbonfibreworks
Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)Supreme Being (2.2K reputation)
Group: Forum Members
Posts: 292, Visits: 4.5K
Hello
Looking at the image it appears that the carbon tubes have increased slightly in diameter where they go over the alloy sections, check with a micrometer and if this is the case for safety reasons do not use the frame. If moisture has made its way between the alloy and carbon corrosion will take place increasing the diameter of the alloy and possibly causing the discolouration you seen in the carbon tube.
Donate the frame to a school or college i am sure they can use it in the engineering/materials dept.
Chris
www.carbonfibreworks.co.uk

http://www.talkcomposites.com/Uploads/Images/97e08777-693c-4af1-a27a-86cf.png
Edited 12 Years Ago by carbonfibreworks
erikrhendrickson
erikrhendrickson
Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)Junior Member (15 reputation)
Group: Forum Members
Posts: 3, Visits: 3
Hey Everyone,

Thanks in advance for your time. Been restoring a 1987 Trek 2500 with full Dura-Ace for my brother's birthday.

The carbon tubes has some bubbling near the lugs just under the clear coat.

http://www.talkcomposites.com/Uploads/Images/816e3102-2075-4e09-9f57-2f60.JPG

http://www.talkcomposites.com/Uploads/Images/f564961a-16a3-49ff-9494-0ae5.JPG

I have the clear sanded off now down to the fibers...was careful not to bite into them.

Do you think this is repairable?  What kind of clear coat should i use...lacquer or enamel?  Any specific recommendations?

Thanks,
Erik
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search