First of all ... a good pump, that can deliver HARD vacuum is essential !!!
I have had very good results with unidirectional, using a wet lay up and a combination of mechanical pressure and vacuum.
I have made I-bars and U-profiles this way .. much stronger and lighter than same size alu profiles..
In fact I used square alu and stainless tubing as moulds for the profiles.
for the I-bars I milled grooves in two pieces of stainless steel, did a wet layup of 200 g standard twill against the mould, and several layers of unidirectional in between.. The finished parts do not have the most perfect surface finish, since i did not spend much time on polishing the steel...

For the U-profile and bars i used an aluminium square tube, and cut one side off, the one with the seam .. (in the mill ...easiest way ..) The sqare tube has a small radius in the cornes, which is a very good thing..  I used a stainless tube as inside mould, I had to mill that smaller in width to fit, and give me the desired thickness of laminate.
After initial layup i simply bagged them and clamped them very hard using a number of C-clamps.. I also found that one must clamp in the middle and work out towards the ends, the slight flex in the tubes i used makes this work rather well 

The longest bar/profile was 400 mm 
If you have trouble wetting the unidir in infusion, maybe you should try to wet out the unidir first and the set up a subsequent infusion?
Maybe my initial success is due to using a combination of unidir and ordinary twill--- hmmm...                
			            
				
			            "Sapere Aude"... Dare to KNOW!
The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...
103% of all people do not understand statistics...
Do not adjust our mind, theres a fault in reality :-)