I have found that cutting Kevlar by all the normal means is extremely difficult.  Worse than that trimming and finishing edges of vacuum bagged parts containing kevlar has never been satifactory.  Kevlar edges always seem to get fuzzy and never look right.  Does anyone have some advice on a) cutting kevlar to produce a clean edge and b) (most importantly) trimming and finishing kevlar edges?


Thank you.

-Kingsley
fgayford
fgayford
Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
KingsleyHill (07/03/2013)
I have found that cutting Kevlar by all the normal means is extremely difficult.  Worse than that trimming and finishing edges of vacuum bagged parts containing kevlar has never been satifactory.  Kevlar edges always seem to get fuzzy and never look right.  Does anyone have some advice on a) cutting kevlar to produce a clean edge and b) (most importantly) trimming and finishing kevlar edges?


Thank you.

-Kingsley


Kevlar is nothing short of a nightmare to trim. You have the same chance of sanding a burlap bag to a high gloss finish as you would with kevlar.

When you embed kevlar try never to have it reach the perimeter where you will actually do the trimming of you carbon panel.

If you do get fibers exposed the only way I have found to push them down is to wet them with resin and then use plastic sheet over the area and tape down firmly with clear packaging tape. Build up resin over the area once cured and you have removed the tape. (light scotch bright first, but do not expose the fibers) Carefully flat out the resin. If you break through your toast again and will have to do the whole thing over again.

If anyone knows how to cut kevlar or better yet drilling a clean whole through it I would really like to know how myself.

Fred
neilb
neilb
Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)Supreme Being (1.3K reputation)
Group: Forum Members
Posts: 107, Visits: 504
you can get the correct scissors to cut kevlar cloth,

some here http://www.shopmaninc.com/cutters.html
wozza
wozza
Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
You can cut kevlar with a decent pair of composite scissors its a slow process, an inch at a time but it does work. If you wet sand edges with 1200's you can get nearly as good a finish as with normal carbon. For drilling I clamp the part between two pieces of perspex, grind the drill bit at a similar angle to that required for sheet metal ie quite steep/pointed.

Regards Warren

Carbon Copies Ltd
fgayford
fgayford
Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
wozza (10/03/2013)
You can cut kevlar with a decent pair of composite scissors its a slow process, an inch at a time but it does work. If you wet sand edges with 1200's you can get nearly as good a finish as with normal carbon. For drilling I clamp the part between two pieces of perspex, grind the drill bit at a similar angle to that required for sheet metal ie quite steep/pointed.

Regards Warren
Thanks for the tips. What is perspex?

Fred
wozza
wozza
Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)Supreme Being (8.5K reputation)
Group: Forum Members
Posts: 688, Visits: 5.4K
Sorry Fred, Perspex is a trade name here in the U.K. It is clear Acrylic sheet. You can often find it used in picture frames in a bargain store (2mm thick) 
Because it is clear you can still see where you have marked the kevlar for drilling. I use the same method on all my composites (where possible) as it prevents "break out" on the back of the hole. It's a trick I learnt as an engineer for drilling holes in very thin shim steel.
Hope that helps.

Warren

Carbon Copies Ltd
Edited 13 Years Ago by wozza
fgayford
fgayford
Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)Supreme Being (6.4K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
wozza (11/03/2013)
Sorry Fred, Perspex is a trade name here in the U.K. It is clear Acrylic sheet. You can often find it used in picture frames in a bargain store (2mm thick) 
Because it is clear you can still see where you have marked the kevlar for drilling. I use the same method on all my composites (where possible) as it prevents "break out" on the back of the hole. It's a trick I learnt as an engineer for drilling holes in very thin shim steel.
Hope that helps.

Warren
Thanks

Good idea! ( here it is called plexiglass )

Fred
brasco
brasco
Supreme Being (2.4K reputation)Supreme Being (2.4K reputation)Supreme Being (2.4K reputation)Supreme Being (2.4K reputation)Supreme Being (2.4K reputation)Supreme Being (2.4K reputation)Supreme Being (2.4K reputation)Supreme Being (2.4K reputation)Supreme Being (2.4K reputation)
Group: Forum Members
Posts: 192, Visits: 305
whew! i learned something today. it wasnt a total waste then Smile
i would NEVER have thought to try this.
.....quietly scribbles note on paper and stuffs into pocket....


fgayford (11/03/2013)
wozza (11/03/2013)
Sorry Fred, Perspex is a trade name here in the U.K. It is clear Acrylic sheet. You can often find it used in picture frames in a bargain store (2mm thick) 
Because it is clear you can still see where you have marked the kevlar for drilling. I use the same method on all my composites (where possible) as it prevents "break out" on the back of the hole. It's a trick I learnt as an engineer for drilling holes in very thin shim steel.
Hope that helps.

Warren
Thanks

Good idea! ( here it is called plexiglass )

Fred



CarbonFiberCreations



tauruck
tauruck
Supreme Being (107 reputation)Supreme Being (107 reputation)Supreme Being (107 reputation)Supreme Being (107 reputation)Supreme Being (107 reputation)Supreme Being (107 reputation)Supreme Being (107 reputation)Supreme Being (107 reputation)Supreme Being (107 reputation)
Group: Forum Members
Posts: 7, Visits: 5
Keeping the fibres away from the perimeter is good advice. Like everyone said cutting Kevlar is difficult. My best method may not suit everyone but I use a box cutter with a brand new blade and trim the part just when it's gone past the green stage. It may require opening the vac bag etc but it beats all the other futile attempts at a fully cured part.Smile
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search