Not a video as I'm a bit camera shy but a step by step guide with pictures.

How to make a Custom Boot/Roof Spoiler

Most of my work is "one off" parts to customer specifications, so I have to make the part from scratch.

I started this project by using Foam Insulation Board (Kingspan) to form the part. A 2400mm x 1220mm x 25mm sheet is around £25 from Builders Merchants/ DIY Stores.

The foil simply peels off leaving the foam which is very easy to cut/shape/sand.
For this project I started with two 1220mm x 200mm strips back to back giving me the required 50mm thickness.
Because the boot lid was curved I taped the first strip to the boot lid with gaffer tape then bonded the second strip to it with a thin layer of "bog" (body filler)
Once the bog is cured the foam will retain the curve of the boot lid.
Now I start shaping the foam to the required profile/shape.
Once I have the shape I seal it with a coat of resin.
Next cover the foam with a layer of 300grm CSM. 
Now I skim the whole part in bog and sand back to a nice smooth finish.
Once happy with the shape/finish I lay up 2 additional layers of 80 grm CSM.
I now have a strong lightweight GRP/foam part.
I then apply 3 coats of high build primer. (this should be enough to level the surface, depending on the primer used)
At this point I can either paint and finish the part or polish the primer and make a mould from it.
Hopefully this will encourage people to have a go at making something from scratch as well as reproducing existing parts.

Regards Warren
 

Carbon Copies Ltd
Edited 12 Years Ago by wozza
brasco
brasco
Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)
Group: Forum Members
Posts: 192, Visits: 305
that was AWESOME!


CarbonFiberCreations



Kevin-Lee
Kevin-Lee
Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)Supreme Being (374 reputation)
Group: Forum Members
Posts: 44, Visits: 2.4K
Hi,

If you think you have seen anything high end, then see this. These guys go from raw PAN precursor to finished parts!

Part 1:



Part 2:



Note that no pre-preg or autoclave is used, its all RTM!

Kev.
Edited 12 Years Ago by Kevin-Lee
fgayford
fgayford
Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)Supreme Being (3.6K reputation)
Group: Forum Members
Posts: 433, Visits: 1.2K
Thanks Scott for compiling these videos, keep them coming.

Is it me or does that rad in the front of the car look a wee bit vulnerable.

Fred
Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
not really a video but a great article with videos in, about CF cars on the carshow in Geneva

Matthieu Libeert
Matthieu Libeert
Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)Supreme Being (7.5K reputation)
Group: Forum Members
Posts: 955, Visits: 3.4K
Thx for sharing those video's, keep sharing them Wink

Matthieu Libeert
Founder MAT2 Composites X Sports
website:
www.mat2composites.com




Bruce
Bruce
Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)Supreme Being (162 reputation)
Group: Forum Members
Posts: 18, Visits: 432
Not really aimed at the tech angle of things but has some nice views of the composite tub 
I am over in Italy next week training for the F12 Berlinetta  I am kinda wishing it was this one Smile

http://www.youtube.com/watch?feature=player_embedded&v=LWvMIJkip7E
brasco
brasco
Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)
Group: Forum Members
Posts: 192, Visits: 305
i am NUTS about my hands. we have to be, no hands/ crippled hands--then we cant do this stuff!  i keep them clean and always wear gloves !


CarbonFiberCreations



baja_patient
baja_patient
Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)Supreme Being (1.2K reputation)
Group: Forum Members
Posts: 135, Visits: 1.6K
No Gloves! Thats crazy! Imagine doing that daily.

Will post some vids soon!

cheers
brasco
brasco
Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)Supreme Being (1.4K reputation)
Group: Forum Members
Posts: 192, Visits: 305
more kevlar in a canoe .they are not using gloves!! eeek!


[YouTube]http://www.youtube.com/watch?feature=endscreen&NR=1&v=orazFL09els[/YouTube]                           


CarbonFiberCreations



Edited 12 Years Ago by brasco
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search