Resin under gelcoat


Author
Message
L2man
L2man
Forum Member (30 reputation)Forum Member (30 reputation)Forum Member (30 reputation)Forum Member (30 reputation)Forum Member (30 reputation)Forum Member (30 reputation)Forum Member (30 reputation)Forum Member (30 reputation)Forum Member (30 reputation)
Group: Forum Members
Posts: 3, Visits: 88
Hi, I’ve been infusing a fairly complex part which is gelcoated - Double gelcoat, then laid up and infused using polyester, quite a thick layup of heavy cloth (6-7mm) and the resin keeps getting through onto the tool side of the gelcoat, and then deforming the gelcoat surface so that it takes ages to get flat again.. any tips?!
Warren (Staff)
Warren (Staff)
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
If the gelcoat is not fully cured it will likely move. Also the styrene in the infusion resin may well be softening the gelcoat making it worse. Also if the gel pre-releases, it will provide an easy path for the infusion resin to flow between the gel and tool surface. 

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search