Group: Forum Members
Posts: 550,
Visits: 27K
|
I have several soric sandwich moulds. Most of the times I use the for elevated temp infusion, but some smaller ones for prepreg too. Most are epoxy based and infused, but some are vinylester/polyester handlaminated. Either way I usually use soric coremat, because it leaves no hex pattern and is much lighter than most other soric variants. 6 layers should be enough to avoid print through anyways. Must be a giant mould if 12 layers of carbon are not stiff enough. For me coremat infuses quite well, but off course needs flow media. Dimensional stability is good, but I tempered them carefully.
|