Skinning Polypropylene


Author
Message
Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Flame treatment is not as straight forward as one might think though, really to do it properly you need special equipment. If you go too far with the flame treatment then the surface tension goes back the other way and you make it unbondable again, so you have to know exactly when the plastic is correctly treated and you have to be able to hit that point consistently over the entire part - not so easy by hand with a blow torch or similar.

Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Very difficult as eluded to above.  You could experiment with flame treatment and skimming with an epoxy adhesive to get a usable surface but its going to be hit and miss. Certainly those approaches aren't likely to work with a resin due to the slow curing speed.  The flame treatment process only really works as it changes the surface reactivity of the plastic for a relatively short period of time. 

Other way to look at it is score it really deeply and heavily to help mechanical locking and wrap the carbon over the edges of the sides or through holes etc to physically mechanically lock the skin in place.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Virtually impossible. Polyolefins like polypropylene are extremely low surface energy, epoxies are just never ever going to bond to them no matter what you do. 

The only way I can see to maybe do it is to create an offset mould that you laminate your carbon into, and then bond it onto your polypropylene using a specialist acrylic adhesive like Permabond TA4610. This obviously isn't going to work for anything but quite simple components, and even then I would question how long it would hold up. My advice - abandon the idea now.
Carbonphoenix
Carbonphoenix
Supreme Being (165 reputation)Supreme Being (165 reputation)Supreme Being (165 reputation)Supreme Being (165 reputation)Supreme Being (165 reputation)Supreme Being (165 reputation)Supreme Being (165 reputation)Supreme Being (165 reputation)Supreme Being (165 reputation)
Group: Forum Members
Posts: 12, Visits: 134
Hey guys,

Been doing a search and the only results are years old and not giving any answers.

I'm looking to skin my PP plastics on my car, and from experience of other parts, PP isn't going to be fun.

So was wondering what process you guys may have worked out now to allow us to skin PP successfully.

Kindest