carguy84 - 1/8/2021 12:37:08 AM
Can you use wax with the XC110 process?  120 degrees isn't too hot for wax?

No you can't, it is too hot. Even most 'high temp' waxes will only handle ~80°. 

There's no need for it, chemical release agents work superbly.

carguy84
c
Supreme Being (76 reputation)Supreme Being (76 reputation)Supreme Being (76 reputation)Supreme Being (76 reputation)Supreme Being (76 reputation)Supreme Being (76 reputation)Supreme Being (76 reputation)Supreme Being (76 reputation)Supreme Being (76 reputation)
Group: Forum Members
Posts: 6, Visits: 176
Can you use wax with the XC110 process?  120 degrees isn't too hot for wax?
chriscnf
c
Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)
Group: Forum Members
Posts: 34, Visits: 2.7K
Fasta - 10/8/2020 8:11:08 AM
chriscnf - 10/8/2020 7:25:38 AM
Fasta - 10/8/2020 6:58:42 AM
chriscnf - 10/8/2020 6:26:23 AM
Warren (Staff) - 10/5/2020 2:32:36 PM
The reason why wax is better as the top coat (or only release coat) for wet lay up and where gelcoats are used, is that semi-permanents can make the surface so slippery that thick gelcoats end up fish-eying and separating on the surface.  So wax "dulls" down the slippery surface a bit making it easier to get the gelcoat on.

As Fasta mentioned it is also good insurance to use 2 release agents like that.  We especially recommend it for taking moulds from patterns where you only get one chance.  PVA is even safer chance of release but it leaves surface marring meaning you need to polish the mould a fair bit to get a good surface.

I'm quite new to semi permanents (Zyvax) and I have been giving the mold a single coat top up after each pull...as much as because I will lose the Zyvax to age as anything. You would need to do a full clean of the mold to apply more semi permanent I assume...but imagine wax coats would give it longer life?

I do exactly that, just keep coating on top. You can even change the release/slip with the different grades from Zyvax/Chemtrend.

Cheers...But do you clean the wax off first before applying a new coat?

For a pre preg mould I use only semi permanent release agents and would continue to add more semi permenant coats.

For a Semi Perm and Wax mould working with wet layups I usually continue to add single waxes each use.
If you wanted to add more semi permanent to the base coats under the wax then safest you should start over with cleaners etc or even a fresh cut polish, new semi permanent 5-6 coats and then wax 5-6 coats initially.

Thanks...appreciate you help and this forum...brilliant

Fasta
Fasta
Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)
Group: Forum Members
Posts: 468, Visits: 3.5K
chriscnf - 10/8/2020 7:25:38 AM
Fasta - 10/8/2020 6:58:42 AM
chriscnf - 10/8/2020 6:26:23 AM
Warren (Staff) - 10/5/2020 2:32:36 PM
The reason why wax is better as the top coat (or only release coat) for wet lay up and where gelcoats are used, is that semi-permanents can make the surface so slippery that thick gelcoats end up fish-eying and separating on the surface.  So wax "dulls" down the slippery surface a bit making it easier to get the gelcoat on.

As Fasta mentioned it is also good insurance to use 2 release agents like that.  We especially recommend it for taking moulds from patterns where you only get one chance.  PVA is even safer chance of release but it leaves surface marring meaning you need to polish the mould a fair bit to get a good surface.

I'm quite new to semi permanents (Zyvax) and I have been giving the mold a single coat top up after each pull...as much as because I will lose the Zyvax to age as anything. You would need to do a full clean of the mold to apply more semi permanent I assume...but imagine wax coats would give it longer life?

I do exactly that, just keep coating on top. You can even change the release/slip with the different grades from Zyvax/Chemtrend.

Cheers...But do you clean the wax off first before applying a new coat?

For a pre preg mould I use only semi permanent release agents and would continue to add more semi permenant coats.

For a Semi Perm and Wax mould working with wet layups I usually continue to add single waxes each use.
If you wanted to add more semi permanent to the base coats under the wax then safest you should start over with cleaners etc or even a fresh cut polish, new semi permanent 5-6 coats and then wax 5-6 coats initially.





chriscnf
c
Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)
Group: Forum Members
Posts: 34, Visits: 2.7K
Fasta - 10/8/2020 6:58:42 AM
chriscnf - 10/8/2020 6:26:23 AM
Warren (Staff) - 10/5/2020 2:32:36 PM
The reason why wax is better as the top coat (or only release coat) for wet lay up and where gelcoats are used, is that semi-permanents can make the surface so slippery that thick gelcoats end up fish-eying and separating on the surface.  So wax "dulls" down the slippery surface a bit making it easier to get the gelcoat on.

As Fasta mentioned it is also good insurance to use 2 release agents like that.  We especially recommend it for taking moulds from patterns where you only get one chance.  PVA is even safer chance of release but it leaves surface marring meaning you need to polish the mould a fair bit to get a good surface.

I'm quite new to semi permanents (Zyvax) and I have been giving the mold a single coat top up after each pull...as much as because I will lose the Zyvax to age as anything. You would need to do a full clean of the mold to apply more semi permanent I assume...but imagine wax coats would give it longer life?

I do exactly that, just keep coating on top. You can even change the release/slip with the different grades from Zyvax/Chemtrend.

Cheers...But do you clean the wax off first before applying a new coat?

Fasta
Fasta
Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)Supreme Being (6.7K reputation)
Group: Forum Members
Posts: 468, Visits: 3.5K
chriscnf - 10/8/2020 6:26:23 AM
Warren (Staff) - 10/5/2020 2:32:36 PM
The reason why wax is better as the top coat (or only release coat) for wet lay up and where gelcoats are used, is that semi-permanents can make the surface so slippery that thick gelcoats end up fish-eying and separating on the surface.  So wax "dulls" down the slippery surface a bit making it easier to get the gelcoat on.

As Fasta mentioned it is also good insurance to use 2 release agents like that.  We especially recommend it for taking moulds from patterns where you only get one chance.  PVA is even safer chance of release but it leaves surface marring meaning you need to polish the mould a fair bit to get a good surface.

I'm quite new to semi permanents (Zyvax) and I have been giving the mold a single coat top up after each pull...as much as because I will lose the Zyvax to age as anything. You would need to do a full clean of the mold to apply more semi permanent I assume...but imagine wax coats would give it longer life?

I do exactly that, just keep coating on top. You can even change the release/slip with the different grades from Zyvax/Chemtrend.





chriscnf
c
Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)Supreme Being (520 reputation)
Group: Forum Members
Posts: 34, Visits: 2.7K
Warren (Staff) - 10/5/2020 2:32:36 PM
The reason why wax is better as the top coat (or only release coat) for wet lay up and where gelcoats are used, is that semi-permanents can make the surface so slippery that thick gelcoats end up fish-eying and separating on the surface.  So wax "dulls" down the slippery surface a bit making it easier to get the gelcoat on.

As Fasta mentioned it is also good insurance to use 2 release agents like that.  We especially recommend it for taking moulds from patterns where you only get one chance.  PVA is even safer chance of release but it leaves surface marring meaning you need to polish the mould a fair bit to get a good surface.

I'm quite new to semi permanents (Zyvax) and I have been giving the mold a single coat top up after each pull...as much as because I will lose the Zyvax to age as anything. You would need to do a full clean of the mold to apply more semi permanent I assume...but imagine wax coats would give it longer life?

Massimiliano
M
Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)
Group: Forum Members
Posts: 167, Visits: 1.1K
Warren (Staff) - 10/5/2020 2:32:36 PM
The reason why wax is better as the top coat (or only release coat) for wet lay up and where gelcoats are used, is that semi-permanents can make the surface so slippery that thick gelcoats end up fish-eying and separating on the surface.  So wax "dulls" down the slippery surface a bit making it easier to get the gelcoat on.

As Fasta mentioned it is also good insurance to use 2 release agents like that.  We especially recommend it for taking moulds from patterns where you only get one chance.  PVA is even safer chance of release but it leaves surface marring meaning you need to polish the mould a fair bit to get a good surface.

Thank you for the additional advice

Warren (Staff)
Warren (Staff)
Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)Supreme Being (37K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
The reason why wax is better as the top coat (or only release coat) for wet lay up and where gelcoats are used, is that semi-permanents can make the surface so slippery that thick gelcoats end up fish-eying and separating on the surface.  So wax "dulls" down the slippery surface a bit making it easier to get the gelcoat on.

As Fasta mentioned it is also good insurance to use 2 release agents like that.  We especially recommend it for taking moulds from patterns where you only get one chance.  PVA is even safer chance of release but it leaves surface marring meaning you need to polish the mould a fair bit to get a good surface.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Massimiliano
M
Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)Supreme Being (2.5K reputation)
Group: Forum Members
Posts: 167, Visits: 1.1K
Fasta - 10/5/2020 6:03:45 AM
Massimiliano - 10/5/2020 5:58:15 AM
Fasta - 10/5/2020 5:50:32 AM
It's not always one or the other.

I use semi permenant release agents on all my moulds including the ones I want to use wax with. Semi perm and then wax on top too.

Thanks!
Why you add wax on top of semi permanent?

The semi permenant gives the mould a safer release and the wax allows you to spray gel coats on to the surface as well as making for a better gloss mould finish. I use this on moulds requiring wet resin layup and I use only semi permenant when working with pre preg and oven cure cooking.

Understood, thank you!

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search