If it is happening with 2 different pre-pregs then it is likely something in your process that is having an impact. As long as the mould is properly post cured then I doubt that is a factor. Try and break down your process to see if there is anything different you are doing. Maybe there is not enough breather around the edge of the part to provide a sufficient air path? As long as your vacuum pump achieves a high level of vacuum then the out of autoclave pre-preg systems are normally fine.