small holes in pattern coat high gloss layer


Author
Message
carlton jacobs
c
Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)
Group: Forum Members
Posts: 5, Visits: 11
ive just applied the finishing coat of pattern coat high gloss over the prepped pattern coat primer on my plug and its got micro holes or pimples in the finished layer theres aproxamtly 3 small holes per square 100mm they are nearly the full depth of the pattern coat and are difficult to sand out,the coat was applied as per video with no runs and a high quality brush.
Lester Populaire
L
Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)Supreme Being (3K reputation)
Group: Forum Members
Posts: 311, Visits: 13K
carlton jacobs - 9/29/2019 9:37:10 AM
ive just applied the finishing coat of pattern coat high gloss over the prepped pattern coat primer on my plug and its got micro holes or pimples in the finished layer theres aproxamtly 3 small holes per square 100mm they are nearly the full depth of the pattern coat and are difficult to sand out,the coat was applied as per video with no runs and a high quality brush.

What is the question? 

carlton jacobs
c
Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)
Group: Forum Members
Posts: 5, Visits: 11
Lester Populaire - 9/29/2019 10:24:38 AM
carlton jacobs - 9/29/2019 9:37:10 AM
ive just applied the finishing coat of pattern coat high gloss over the prepped pattern coat primer on my plug and its got micro holes or pimples in the finished layer theres aproxamtly 3 small holes per square 100mm they are nearly the full depth of the pattern coat and are difficult to sand out,the coat was applied as per video with no runs and a high quality brush.

What is the question? 



carlton jacobs
c
Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)Forum Member (46 reputation)
Group: Forum Members
Posts: 5, Visits: 11
Lester Populaire - 9/29/2019 10:24:38 AM
carlton jacobs - 9/29/2019 9:37:10 AM
ive just applied the finishing coat of pattern coat high gloss over the prepped pattern coat primer on my plug and its got micro holes or pimples in the finished layer theres aproxamtly 3 small holes per square 100mm they are nearly the full depth of the pattern coat and are difficult to sand out,the coat was applied as per video with no runs and a high quality brush.

What is the question? 


why are the holes in the finishing coat,how can I avoid them in the future
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
Depends what has caused them, we would need to see a picture.
Warren (Staff)
Warren (Staff)
Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)Supreme Being (23K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Pictures would greatly help.  Do you mean pinholes or large holes where the resin has separated? (aka fisheyed).

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search