You have to consider your flanging and barriers. Vacuum processed moulds like pre-preg and infusion require solid flanges, they cant be temporary flanges as you might make for a wet-laid Unimould tool.
So realistically, you cant use vacuum processed moulds to replicate an OEM vehicle panel. To do so, you would first need to build wet-laid moulds in the regular fashion (although you can get away with doing cheaper 'splash' moulds), then use those moulds to remake a male version of the panel but this time with flanges built onto it. Then you can use these new patterns to make resin infused or pre-preg moulds. By the time you've gone to all this effort, a simple wet-laid epoxy mould would be significantly cheaper and easier.
I do this sort of thing fairly often for production moulds, but never for a once off.
|