EL2 Laminating resin mixing problem


Author
Message
Steve Broad
Steve Broad
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 408, Visits: 4.1K
Rich (Staff) - 10/23/2018 4:30:17 PM
I was just going to say Steve, it would have been road transport because of the DG nature of the materials.

Ah, good point. But at least that possibility has been eliminated :-)

Rich (Staff)
Rich (Staff)
Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)
Group: Administrators
Posts: 167, Visits: 4.6K
I was just going to say Steve, it would have been road transport because of the DG nature of the materials.
catacls
c
Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)
Group: Forum Members
Posts: 10, Visits: 180
Steve Broad - 10/23/2018 3:59:55 PM
Warren (Staff) - 10/23/2018 3:31:33 PM
Interesting point Dravis. Although ambient temperatures are not that low yet, you never know if the parcel has been left in cold storage or next to a chilled/frozen reefer or similar in the transit depots.


Or in the hold of the plane transporting the hardener to Romania, although this rarely goes below 7 deg C.

This parcel wasn t transported by plane.

Steve Broad
Steve Broad
Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)Supreme Being (4.9K reputation)
Group: Forum Members
Posts: 408, Visits: 4.1K
Warren (Staff) - 10/23/2018 3:31:33 PM
Interesting point Dravis. Although ambient temperatures are not that low yet, you never know if the parcel has been left in cold storage or next to a chilled/frozen reefer or similar in the transit depots.


Or in the hold of the plane transporting the hardener to Romania, although this rarely goes below 7 deg C.
Warren (Staff)
Warren (Staff)
Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
Interesting point Dravis. Although ambient temperatures are not that low yet, you never know if the parcel has been left in cold storage or next to a chilled/frozen reefer or similar in the transit depots.


Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Dravis
Dravis
Supreme Being (7.9K reputation)Supreme Being (7.9K reputation)Supreme Being (7.9K reputation)Supreme Being (7.9K reputation)Supreme Being (7.9K reputation)Supreme Being (7.9K reputation)Supreme Being (7.9K reputation)Supreme Being (7.9K reputation)Supreme Being (7.9K reputation)
Group: Forum Members
Posts: 592, Visits: 1.9K
Hi!

Is it possible that only the AT30 Fast hardener container in question has been partially frozen during transport (Air freight?)
I had a partly used AT30 fast hardener that was accidentally partially frozen last winter, I thawed it out and did a test on it and had the exact same problems described here.

I have to admit that that particular container of hardener was past its 12 months shelf life, but I had two containers delivered at the same time, and the one that was kept cold, but not frozen worked fine.
As a matter of fact I just used the remaining of this last container of AT30 Fast, which by now must be at least 2 years old and it worked just fine. It has darkened quite a bit, so I only used it for non-structural, non cosmetic use (Quick&dirty CF Mould :-) )

Could the  particular container of  Fast hardener have been contaminated with water? And would that combined with freezing explain the severe problems "catacls" seems to have?


"Sapere Aude"... Dare to KNOW!

The written word is the only truly efficient vehicle for transmitting a complex concept from mind to mind...

103% of all people do not understand statistics...

Do not adjust our mind, theres a fault in reality :-)
catacls
c
Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)
Group: Forum Members
Posts: 10, Visits: 180
Warren (Staff) - 10/22/2018 11:56:04 AM
I have checked the batch details you have given and it all seems fine from the current batch which we have tested and use in house so I am baffled as to what is going on here.

As you say youve controlled the temperature and humidity.  If you've got up to 35C it should cure quicker and better than normal.

The fact you get so much amine blush and delamination concerns me  - are you mixing by volume or by weight and I presume following the standard mixing ratio and not varying it?  So much amine blush almost sounds like you have lots of uncured hardener in the mix.
Thank you for your reply. The mixing is always done by weight. There was nothing wrong with the slow hardner, from the 5 kg set I have used it all. And more so, i have managed to cure the resin with a modified aliphatic amines hardner from another brand that uses the same 100:30 ratio and the cured resin was ok.

Warren (Staff)
Warren (Staff)
Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)Supreme Being (34K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
I have checked the batch details you have given and it all seems fine from the current batch which we have tested and use in house so I am baffled as to what is going on here.

As you say youve controlled the temperature and humidity.  If you've got up to 35C it should cure quicker and better than normal.

The fact you get so much amine blush and delamination concerns me  - are you mixing by volume or by weight and I presume following the standard mixing ratio and not varying it?  So much amine blush almost sounds like you have lots of uncured hardener in the mix.


Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
catacls
c
Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)Supreme Being (187 reputation)
Group: Forum Members
Posts: 10, Visits: 180
As I previously stated, my humidity and temperature are controled. The dehumidifier kicks of at 50% rh usually, for this resin I have gone as far as 35 with some great efforts and still no improvement. The temperature also is controled by a thermostat according to my needings. I am more than happy to send the hardner back if easycomposites pays for shipping. I expect nothing else in return, otherwise I will throw it away anyways.
The amine blush goes deep in the laminating layer, after i wash it off with water and soap, when I sand it white spots appear on the surface. Not to mention if I apply subsequent layers at the tacky stage, they will delaminate immediatly. 
And to eliminate all doubts, all the containers are very well kept, in their original one, and the resin was ordered 2 weeks ago. Please do not ask about this again.

Rich (Staff)
Rich (Staff)
Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)Supreme Being (2.1K reputation)
Group: Administrators
Posts: 167, Visits: 4.6K
To pick up on one of your other posts as well, each batch of hardener is around 200-400kg and so a batch issue (which would be unheard of) would affect dozens of customers. We also use the AT30 Fast in our production of Composite materials so I'm confident that the material is okay but to be sure, could you kindly confirm the batch number on your container (it is found next to the barcode)? We can then double check the batch against our records accordingly.
Edited 8 Years Ago by Rich (Staff)
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search