Storing resins and gel coats in hot temps


Author
Message
drippy
drippy
Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)
Group: Forum Members
Posts: 32, Visits: 388
Hanaldo - 8/9/2018 4:30:25 AM
I actually store a lot of my products in the freezer at -18C. My more expensive polyester/vinylester based coatings like tooling gelcoat, Duratec primers/top-coats, etc. Make sure they are really well sealed so no moisture gets into them and they aren't worried at all. Let them defrost for a day before using them and they last virtually forever.

My cheaper and easier to obtain products like regular gelcoat and laminating resins etc. it doesnt worry me as much if they go off before I use them, so they live in the shed. I havent had any of them go off before I finish them yet though.

That's really good to know. I can get freezers for a ton cheaper than fridges.. I'll just keep a single 5 gallon pail of each of what I use everyday and put the rest in a freezer.

Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
I actually store a lot of my products in the freezer at -18C. My more expensive polyester/vinylester based coatings like tooling gelcoat, Duratec primers/top-coats, etc. Make sure they are really well sealed so no moisture gets into them and they aren't worried at all. Let them defrost for a day before using them and they last virtually forever.

My cheaper and easier to obtain products like regular gelcoat and laminating resins etc. it doesnt worry me as much if they go off before I use them, so they live in the shed. I havent had any of them go off before I finish them yet though.
drippy
drippy
Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)
Group: Forum Members
Posts: 32, Visits: 388
Hanaldo - 8/8/2018 6:13:03 AM
The epoxies will be fine, it's the styrene based resins that will suffer. Vinyl esters are especially sensitive. That said, I've only ever had Duratec products go off on me in the space of a couple of months of Australian summer. The VE infusion resin I had also went solid, but that took about 6 months.

That is some good info to start with thank you!  I think I might split my drum up of VE resin into 5 gallon pails and buy a cheap used top loading fridge and gut it out and put the pails in there and set the fridge at it's warmest temp. Should be interesting to see how it works. It will take me about 8 months to use the drum so if I can get more life out of it this way and store maybe 40 gallons colder I can get the whole life of the drum. 

Hanaldo
Hanaldo
Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)Supreme Being (35K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
The epoxies will be fine, it's the styrene based resins that will suffer. Vinyl esters are especially sensitive. That said, I've only ever had Duratec products go off on me in the space of a couple of months of Australian summer. The VE infusion resin I had also went solid, but that took about 6 months.
drippy
drippy
Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)Supreme Being (471 reputation)
Group: Forum Members
Posts: 32, Visits: 388
Well it is summer which means it's hot!  Well 115 degrees fahrenheit. Making where I store my materials around 105-120 degrees depending where the sun is sitting. Am I gonna have issues with my materials over an extended amount of time away from the normal shelf life?  I am using clear poly gels, tooling poly and VE tooling gel coat. Infusing with VE resin and west systems epoxy. I don't use a lot of epoxy and that can be stored in a cooler area but the drums of stuff really can't fit in a cooler section.
Edited 8 Years Ago by drippy