Hi Treasure,
800 grit is far too coarse to get a good gloss finish from. You need to as a very minimum bring the lacquer up to a 1200 grit wet or even better 1500 grit wet finish before you can use a polishing compound.
The polishing compounds only have a very fine cutting ability so with 800 grit it simply cannot cut out the coarse scratches hence it still looks matt. With 1500 grit, the scratches are minute and within the capability of the polish to remove to bring it to a gloss.
Assuming you haven't gone right through the lacquer, you should be able to start again at 800 grit then work back to 1500 grit and polish to a high gloss.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|