Group: Forum Members
Posts: 237,
Visits: 4.8K
|
You can use it without release,we use to make the turbo/intercooler pipes for the Renault v6 on the f1 cars that very way many years ago
Also has the advantage you can put 1 ply in your mould as your cosmetic ply the others can be laid around your silicone former with all the material joins staggered (butt joints of course)
Obviously silicone tube was hollow an was internally bagged
Current practice everyone uses 3d printed pipes
they can be rubbed down to a perfect Finnish,sealed an released
As you cook an have a dwell at 80 deg,just as your resin starts to flow an gel the 3d also softens enough to allow consolidation of the part
once cured an stripped from the mould heat to 140 an the 3d turns to a rubber like consistency and is easily pulled from some very complicated pipe shapes
|