Been making up a mold for a racing kayak heel rest and a seat and thought I would post up my progress here. The images are not the best quality but hope you get the idea.

http://www.talkcomposites.com/Uploads/Images/dc04f156-efc6-4fa2-ba13-5f41.jpg     http://www.talkcomposites.com/Uploads/Images/1ceefa4b-452f-42b2-8828-04e3.jpg



The front and back of the original made out of glass.  I'm going to make some adjustments to this so that it will come out the mold easier.  I flanged this up with some old mdf board and waxed it with some filleting wax around the edges to seal it.

I forgot to take some pictures of the plug flanged but I backed up the plug with a homemade epoxy gel coat out of EC epoxy resin and fumed-silica.  This has given a nicy shiny finish to the mold surface and I am pretty pleased with how it turned out.

Layup of the mold was 100g glass tape, 200g carbon, 1mm spherotex core, 200g carbon, 100g glass tape.  This has given a strong mold if not a bit over the top.  

Bit expensive to complete large molds this way but hopefully they will last the course!  I will follow up in a few hours with pictures of the mold and the seat!