Easy-lease and wet layup - fish eye problems


Author
Message
fatbaldbloke
fatbaldbloke
Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)Junior Member (20 reputation)
Group: Awaiting Activation
Posts: 2, Visits: 15
I'm having a bit of a 'mare.  I'm trying to make a flat carbon panel.  The "mould" is a sheet of glass.  I've coated it with easy-lease but when I put on the first layer of resin (EL2 fast) it fish-eyes straight away.  There seems no point letting the first layer dry to a tacky state as it's just pools of resin.  Should I just get on with laying the fibre straight on the wet resin.
I have also tried using the epoxy gel coat for the first layer but still had some fish-eyes plus as it went tacky it appeared to crystalise.  Wasn't right at all.  (Is it possible for gel coat to go off with storage in a fairly cold garage?)  It's also not particularly clear, it's a sort of smoky blue.
Not sure where to go now to get a decent wet layup flat sheet technique.  Any help gratefully received. 
Reply
MikeH
MikeH
Forum Guru (56 reputation)Forum Guru (56 reputation)Forum Guru (56 reputation)Forum Guru (56 reputation)Forum Guru (56 reputation)Forum Guru (56 reputation)Forum Guru (56 reputation)Forum Guru (56 reputation)Forum Guru (56 reputation)
Group: Forum Members
Posts: 6, Visits: 13
Update!Applied 2 coats of McGuires wax, perfect now no fish eyes and great release from molds. 
Thanks
GO