Group: Forum Members
Posts: 363,
Visits: 3K
|
unless someone has developed a super resin it does not exist, the way the resin builds it's strength requires heat to create the molecular chains within.
What you can try to find is a resin which you can cure at 40-50deg in the oven with the plug then demould and post cure to the temp you require. You need a resin which will not soften under high temperature post cure.
Or better still find an out of autoclave pre-preg which will do the above, look at the tooling pre-pregs as these often have a low initial cure temperature exactly for your situation.
|