Vacuum Gauge Precision (can't pull full vacuum)


Author
Message
H4RTM4N
H4RTM4N
Supreme Being (111 reputation)Supreme Being (111 reputation)Supreme Being (111 reputation)Supreme Being (111 reputation)Supreme Being (111 reputation)Supreme Being (111 reputation)Supreme Being (111 reputation)Supreme Being (111 reputation)Supreme Being (111 reputation)
Group: Forum Members
Posts: 7, Visits: 203
Hi all,

My name is Andreu and I'm new to this forum. I've just received my order from EC and I'm already trying to make my own carbon fibre parts using resin infusion.

For the first trial I wasn't concerned about the final quality of the part (a simple plate) as I only wanted to be familiar with the process. However, I noticed I couldn't reach 'full' vacuum. Instead, the vacuum gauge was stuck at -29Hg (0.98+ bar). I closed all the leaks in the vacuum bag but I kept having that remaining pressure inside. In order to be sure of that, I connected the vacuum pump to the resin catch-pot only. The hose that usually comes from the resin catch-pot was clamped so the vacuum was only made inside the catch-pot. When I pulled vacuum from the pot, I obtained the same result. 

Taking into account that I live in Barcelona and my house is <100m above sea level, I wonder if my equipment is all right or not. In other words, I want to know if the the vacuum gauge is simply not representing the reality inside the bag because of its precision. I can imagine 2 possible answers to the question:

- YES, the equipment is just fine. The precision of the vacuum gauge of the resin catch-pot is somewhat near to 2mbar and that is why I obtain these 0.98bar.
- NO, there's something wrong. You should obtain -1bar (-30Hg), which in reality represents the advertised 99.995% vacuum.

Could you please help my clarify this issue? 

Thank you a lot and good luck to everyone!

Regards,

Andreu

 
Edited 13 Years Ago by H4RTM4N
Replies
Warren (Staff)
Warren (Staff)
Supreme Being (25K reputation)Supreme Being (25K reputation)Supreme Being (25K reputation)Supreme Being (25K reputation)Supreme Being (25K reputation)Supreme Being (25K reputation)Supreme Being (25K reputation)Supreme Being (25K reputation)Supreme Being (25K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
An accurate guage will only tell you accurately what the leak has dropped to - which is irrelevant.

Its the fact you have a leak full stop thats important, and the cheapo gauge will tell you theres a leak just as effectively.

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
morepower
morepower
Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)Supreme Being (1.8K reputation)
Group: Forum Members
Posts: 242, Visits: 1.2K
Although I have found there is a difference in total vacuum pulled between two different pumps. So having a good gauge will also tell you if the pump is not as efficient and needs an oil change or replacing.. A gauge which is not so accurate will have you allowing for a cheap gauge and thinking the difference is down to many factors but ultimately leave you thinking the gauge is cheap and it is at fault not the pump ect... 

Having said that my fluid filled gauge we still less than £30 and I would rather have a good gauge then estimate or second guess a cheap one..
Edited 13 Years Ago by morepower
Matt (Staff)
Matt (Staff)
Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)Composites Expert (Staff) (10K reputation)
Group: Forum Members
Posts: 680, Visits: 1.9K
Thanks for the interesting feedback everyone.

Warren made some valid points but I agree that there are situations where a very accurate vacuum gauge is called for. For day-to-day applications a simple vacuum gauge is all that's required, particularly if you're not trying to compare two pumps etc. and of course changes in atmospheric pressure will affect the pressure shown on the gauge anyway which is why we often suggest that people don't rely too heavily on the vacuum gauge as an absolute truth and instead learn to read other signs (like the pump's sound) as indicators of leaks etc. No vacuum gauge I've ever used will indicate the minute difference in pressure between a tiny leak and no leak in the way that opening and closing the valve to the vacuum pump will and so I understand why Warren was emphasizing that point.

I'll certainly look into sourcing some high-end vacuum gauges as an upgrade option for our product range. 'morepower' is quite right that a good gauge doesn't need to cost the earth.

Best regards, Matt

Matt Statham
Easy Composites / Carbon Mods - Technical Sales
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
H4RTM4N - 13 Years Ago
fgayford - 13 Years Ago
H4RTM4N - 13 Years Ago
fgayford - 13 Years Ago
prairiecustomcomposites - 13 Years Ago
fgayford - 13 Years Ago
matthieutje65 - 13 Years Ago
fgayford - 13 Years Ago
Warren (Staff) - 13 Years Ago
             Thanks for the feedback people!
H4RTM4N - 13 Years Ago
Warren (Staff) - 13 Years Ago
morepower - 13 Years Ago
alebassa - 13 Years Ago
Warren (Staff) - 13 Years Ago
morepower - 13 Years Ago
Matt (Staff) - 13 Years Ago
brainfart - 12 Years Ago