Group: Forum Members
Posts: 311,
Visits: 13K
|
Even tho Hanaldo is certainly right with the PC and ABS being hard to bond to, there is a fairly easy solution to this that works at least on ABS. Ski sidewalls are made from ABS more often than not and are usually flame treated to improve bonding.
First clean the surface with IPA. then with fresh 60 grit sandpaper key the surface. use a Bunsen burner and "paint" over the whole area. you can check if the surface tension changed by applying a drop of water which should not bead up but wet a big area.
Hope this helps!
|