Was starting a mold today and got terrible alligatoring when I applied the second coat of gel coat.

Is this only caused because I applied the second coat too soon? Or could there have been other factors causing this mess?


Sorry the image is inverted, I'll fix it when I'm on a computer.
Replies
beliblisk
b
Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)
Group: Forum Members
Posts: 53, Visits: 2.8K
When i apply gelcoat i do it really thin on first brush up just to make sure i cover everything and then make another pass adding to normal thickness (probably close to 1mm).Second aplication is in thickness the same as firts. This way i never had any problems so far.

Good luck
Edited 5 Years Ago by beliblisk
Hanaldo
Hanaldo
Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)Supreme Being (21K reputation)
Group: Forum Members
Posts: 2.5K, Visits: 28K
beliblisk - 6/14/2020 6:56:59 PM
When i apply gelcoat i do it really thin on first brush up just to make sure i cover everything and then make another pass adding to normal thickness (probably close to 1mm).Second aplication is in thickness the same as firts. This way i never had any problems so far.

Good luck

*without letting it cure in between*, correct? 

This is what I do as well as it takes advantage of the thixotropic properties of the gelcoat - thin when brushing, thick when left to sit. Brush it on so that everything is covered. By the time everything is covered, the gelcoat you've brushed on already has returned to its thickest state and you can brush over the top of it and disturb it less, allowing you to build thickness easier than if you tried to go straight to full thickness.

But don't let it cure in between that first thing coat and the second thin coat, it is all done in one application.

beliblisk
b
Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)Supreme Being (563 reputation)
Group: Forum Members
Posts: 53, Visits: 2.8K

Correct. Just thin film followed right away with thicker second application (after about 2h folowed by "true" second layer). 

GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
AlpineCoupe - 5 Years Ago
oekmont - 5 Years Ago
AlpineCoupe - 5 Years Ago
beliblisk - 5 Years Ago
Hanaldo - 5 Years Ago
beliblisk - 5 Years Ago
AlpineCoupe - 5 Years Ago
Hanaldo - 5 Years Ago
beliblisk - 5 Years Ago
AlpineCoupe - 5 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search