Ambient temp is the problem, gelcoat won't cure at 10° with 2% catalyst. Even with 5% catalyst it wouldnt cure, ambient temp needs to be an absolute minimum of 15° to work with gelcoats.
Can you warm your working environment or even just the plug up at all? Theres a good chance the gelcoat will still cure if you can get it up to 30 or 40°.
|