I have bonnet from.my beetle.In general it have no frame underneath, but it have big kind of lip around.
I think about two options.
First lay up more layers in that area around.
Second lay up CF tape. 
Any suggestions what will give better result?

Matt (Staff)
Matt (Staff)
Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)Composites Expert (Staff) (8.4K reputation)
Group: Forum Members
Posts: 680, Visits: 1.9K
I'm not quite sure I understand what you mean by a better result? - Assuming you mean what would give the most strength in this area then there wouldn't be any different between multiple layers of woven carbon fibre tape and multiple layers of woven carbon fibre cloth, they're really just two different formats of the same thing. Therefore, given the large size of this 'lip' then I'd suggest that woven carbon fibre cloth would be the most practical way to reinforce this area.

The shape, size and way this panel is mounted might mean that it really doesn't need much by way of additional stiffness and certainly the convex dome-like shape will naturally be a strong shape anyway. If you did find that after making it as a single skin that needs some additional stiffness then you could always add some 3mm closed cell foam sandwiched underneath another layer of carbon fibre. This could be done after the main part was made and simply wet-laid on and then vacuum bagged down.

Matt Statham
Easy Composites / Carbon Mods - Technical Sales
Classicarbon
C
Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)
Group: Forum Members
Posts: 86, Visits: 639
Matt (Staff) - 2/17/2020 8:08:15 AM
I'm not quite sure I understand what you mean by a better result? - Assuming you mean what would give the most strength in this area then there wouldn't be any different between multiple layers of woven carbon fibre tape and multiple layers of woven carbon fibre cloth, they're really just two different formats of the same thing. Therefore, given the large size of this 'lip' then I'd suggest that woven carbon fibre cloth would be the most practical way to reinforce this area.

The shape, size and way this panel is mounted might mean that it really doesn't need much by way of additional stiffness and certainly the convex dome-like shape will naturally be a strong shape anyway. If you did find that after making it as a single skin that needs some additional stiffness then you could always add some 3mm closed cell foam sandwiched underneath another layer of carbon fibre. This could be done after the main part was made and simply wet-laid on and then vacuum bagged down.

Great thanks.I thought that the shape will give enough stiffness like you said. It's my first set up so I'm not sure how.many layers will be the right number.Buy if I can add things after infiusion that's perfect.

Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
You will be surprised how much the curvature helps with stiffness.  A typical bonnet or boot skin, which is relatively flat, without a core may have 6 or 7 layers of a 210gsm cloth - less if an additional support frame or foam core is used.  Something like this you might be able to use less.  Perhaps a single layer of a 210gsm cloth on the surface, and then a couple of layers of 450gsm cloth to back up.  The 210gsm cloth is around 0.25mm thick and the 450gsm 0.5mm thick per layer so you would end up with something just over a mm thick.  With the double curvature that should certainly hold it's shape and have a nice bit of stiffness.  If it has a bit too much flex or twist, you could add some foam core material as Matt suggested above. 

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
Classicarbon
C
Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)Supreme Being (768 reputation)
Group: Forum Members
Posts: 86, Visits: 639
Warren (Staff) - 2/18/2020 11:03:52 AM
You will be surprised how much the curvature helps with stiffness.  A typical bonnet or boot skin, which is relatively flat, without a core may have 6 or 7 layers of a 210gsm cloth - less if an additional support frame or foam core is used.  Something like this you might be able to use less.  Perhaps a single layer of a 210gsm cloth on the surface, and then a couple of layers of 450gsm cloth to back up.  The 210gsm cloth is around 0.25mm thick and the 450gsm 0.5mm thick per layer so you would end up with something just over a mm thick.  With the double curvature that should certainly hold it's shape and have a nice bit of stiffness.  If it has a bit too much flex or twist, you could add some foam core material as Matt suggested above. 

You right, but then cos lid is from classic car and you not consider speed more than 90mph it might don't need that many layers. 
And this lid got only under frame on the top originally.
I think extra stiffness is coming from the"L" shape lip around.
Ignore the red line.

Warren (Staff)
Warren (Staff)
Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)Supreme Being (22K reputation)
Group: Administrators
Posts: 2.5K, Visits: 8.5K
The L shape lip will certainly add a significant amount to the stiffness of the part.  

Warren Penalver
Easy Composites / Carbon Mods - Technical Support Assistant
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search