Bubbles on sharp corners


Author
Message
raygun
r
Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)
Group: Forum Members
Posts: 22, Visits: 126
This is my first time working with fiberglass. I'm working on a small fender for my race car. Ultimately, I'd like to do these and some other parts in carbon, but it seemed wise to spend some time practicing and learning with cheaper materials.
I made a mold of an existing fender using tooling gelcoat, fiberglass cloth and polyester resin. That worked really well, and I'm happy with the mold.
But, my first part did not turn out so well. In most places where there are relatively sharp bends, I'm getting large (1"-2" long) voids, which I assume are due to air bubbles forming where the 225g fiberglass cloth separates from the mold while curing.

Any suggestions on how to address this? Should I be using CSM instead of cloth? I've seen mention of others using spray adhesive to keep the glass in place, but I'm not sure how that might affect the mold release. (I'm using spray PVA.)

Original part (which was cleaned up after this shot, before working on the mold):


Top outside edge. The voids are clearly visible.



Leading edge with some clay and stuff still hanging on.



Replies
scottracing
scottracing
Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)Supreme Being (3.9K reputation)
Group: Forum Members
Posts: 460, Visits: 5.2K
What process are you using to make the parts? It's definitely due to bridgining of the material in the corners, you need to ensure you force the material into the corners as a vac bag will.not give enough.
raygun
r
Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)Supreme Being (257 reputation)
Group: Forum Members
Posts: 22, Visits: 126
Thanks for the response.

As I said, I'm very new to this. But, basically:

1. Clean the mold
2. Spray PVA- thin layer followed by a thicker layer, let it set
3. Brush a layer of resin into the mold
4. Apply a layer of cloth. Roll it down, push it into corners with a corner rolling tool, get all the air out that I can
5. Apply another layer of resin, another layer of cloth, do three layers of cloth in total.

I'm sure  I'm doing many things wrong. I just don't know what they are. I'm not vacuum bagging, though I'm considering it and researching how that works.

Any insight would be appreciated.



GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View
Threaded View
raygun - 6 Years Ago
scottracing - 6 Years Ago
raygun - 6 Years Ago
Hanaldo - 6 Years Ago
raygun - 6 Years Ago
oekmont - 6 Years Ago
MarkMK - 6 Years Ago
raygun - 6 Years Ago

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search