Hi
I made a carbon front fender for my Husqvarna 701 Supermoto in a four part mould. The part of the mold that depicts the assembly area is cast from polyurethane.
 
I fill the mounting area of the front fender with a thickened resin before vacuuming.
I use about ¾ teaspoon chopped carbon fibre strands on 65 g of resin.

The result looks neat, but the assembly area is more brittle than I expected.
It sometimes breaks when I drill it. I am afraid it will break in rough use.
If possible, I do not want to build a new mould.
Any suggestions?
Regards
Frank

Reply
George Sychrovsky
George Sychrovsky
Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)Supreme Being (228 reputation)
Group: Forum Members
Posts: 24, Visits: 1.6K
Frank - 12/24/2018 10:25:29 AM
Hanaldo - 12/24/2018 9:46:38 AM
It's a nice approach, I like it. 

Are you vacuum degassing the cast section? It looks like it is full of air bubbles, which will drastic lower its strength.


Hi Hanaldo.
No, I did not degass it.
I mixed the chopped strands into the resin after mixing the AT30 in it.
Frank

I would make a separate angle like carbon part and then bond it in ,



---------------------------------------------------------------------
Disclaimer opinions of others will vary depending on what they are selling
GO

Merge Selected

Merge into selected topic...



Merge into merge target...



Merge into a specific topic ID...




Threaded View

Similar Topics

Reading This Topic

Explore
Messages
Mentions
Search