which is the best way to seal the wood surface before making the mould ?
Reply
MAVERICK
MAVERICK
Supreme Being (251 reputation)Supreme Being (251 reputation)Supreme Being (251 reputation)Supreme Being (251 reputation)Supreme Being (251 reputation)Supreme Being (251 reputation)Supreme Being (251 reputation)Supreme Being (251 reputation)Supreme Being (251 reputation)
Group: Forum Members
Posts: 27, Visits: 39
Not sure what the 'best' way is but i can tell you how I've done it.

1 way is to paint it with car paint... not the rattle-can stuff but proper 2-pack, the filler primer type is the one to go for... this builds a thick coat coat that's pretty easy to sand and polish. you just stick you release agent onto that and you good to go.

the other way I have used that worked pretty well was to use shellac sanding sealer, I think it's normally used for furtinture and stuff, you can get it from B&Q, a few coats of that and a sand and buff and again you can go straight on with release agent.

basically I think anything that seals the surface and allows for a bit of a polish will work as long as it doesn't react with the resin, always try a test peice beofre you go and get your pattern stuck in the mould!