There isn't really anything more sticky as such than the basecoat. You will find that if you use a spray tack, often the glue will begin to loose it's hold as you wet the fabric out with resin.
What you can do on tight corners is to place the fabric where it needs to be then leave the clear coating resin for another few hours time. It will give the basecoat a bit more time to set and grip the fabric a bit better. If that doesnt work you can use a small plastic or similar former the same shape as the corner to press the fabric into the corner then leave it there while the basecoat sets. Release coat the former or use a bit of polypropylene sheeting or packing tape on it so it does not stick to any resin that squeezes through the fabric.
Warren Penalver Easy Composites / Carbon Mods - Technical Support Assistant
|